PETG Support for PLA: Interface Tests & B2B Settings

TL;DR: PETG Support for PLA Works as a Thin Interface with Controlled Contact

PETG support for PLA works because the tested PLA/PETG interface has low adhesion under the right print conditions. In a 2025 study using a Prusa XL, the standard PLA/PETG butt joint measured 1.6 MPa, compared with 50 MPa for the solid PLA reference. On the Snapmaker U1, our starting profile uses three PETG interface layers and 0 mm Top Z; validate the same pair on the target printer before releasing a production profile. Set the purge volume for the switch back into the model material.

Best optionPETG interface layers on a PLA support base, with PETG on its own tool-changer tool. The 0 mm Top Z / 3-layer starting profile is U1-specific.
When not to use itTPU parts (PETG bonds strongly to TPU) and PA-CF on 80–100 °C beds; use PLA for TPU, PA/PET breakaway for PA-CF.
Key specificationFlush back into PLA: 300 mm³ passed in our lot test, 400 mm³ released; back into PETG: 800 mm³. PETG dried 65 °C × 8 h.
Verify the supplierBatch IDs on both spools, COA moisture, and a tensile bar across the material switch.
Procurement warningAt 800/800 mm³ on one nozzle, an interface layer burns about 2 g of purge. Prusa publishes about 13 mg per INDX change; SSSray measured 11.6 mg per change on its PLA ↔ PLA INDX coupon.

1. Does PETG Support for PLA Work? Why the Two Plastics Release Cleanly

Yes. In the 2025 study cited below, the tested PLA/PETG standard butt joint had the lowest tensile strength among the material combinations in that study, at 1.6 MPa. A PETG interface can support a PLA overhang and release during removal, but the result is not automatic: interface temperature, contact pressure, contamination, geometry and the specific filament grades all affect peel behavior.

Think of two dry sheets of paper that slide apart; add a smear of glue and they tear instead. Your settings decide how much “glue” sneaks in.

Chemistry: why PLA and PETG barely bond

A strong interface depends on intimate contact, thermal history and sufficient time for polymer-chain interdiffusion before the material solidifies. Zatloukal and colleagues discuss these mechanisms and report that the tested PLA/PETG standard joint measured 1.6 MPa, while the tested PC/PETG standard joint measured 15.2 MPa. The authors attribute the weaker PLA/PETG result in part to differences in molecular structure, polarity and processing temperature. These are results for the study’s materials and joint designs, not universal strength values for every PLA/PETG grade. Figure 1 compares the reported measurements.

Tensile strength of printed joints and solid references (MPa)

Figure 1. Mean tensile strength, Zatloukal et al., Materials 2025: Prusa XL, ISO 527-1 type 1A, n = 10 per condition, 0.2 mm layers, 100% infill, PLA 225 °C / PETG 250 °C nozzle, shared 70 °C bed. Scale 0–50 MPa. Amber: release window. Teal: bonded joints. Grey: single-material references.

Contact and moisture: when a release layer becomes a weld

In the study, the increase from 1.6 to 25.4 MPa came from a deliberately engineered interlayer-bonding design that increased contact and applied pressure. It does not show that routine over-extrusion, a hotter nozzle or a slower pass will produce the same strength. In support printing, excess contact or heat can still increase adhesion, while moisture can shift the result in either direction. Snapmaker’s U1 guide specifically warns about damp support material.

PETG filament spool in a drying cabinet beside a peel-test coupon.
Procurement implicationBuy the interface material against a moisture value, not a color name.
Mistake to avoidTreating “PLA and PETG don’t stick” as a law; over-squish, heat and wet filament raise the bond.
How to verifyPrint a 40 × 40 mm peel coupon and a tensile bar printed across the material switch.

2. PLA Support for PETG: The Reverse Pair Works, but the Flush Rules Change

You can use PLA as support for PETG, but this is the less forgiving direction. PLA residue in the nozzle can weaken the next PETG layers, and the first PETG layer printed onto a cool PLA interface can string instead of bonding to the interface.

PETG specks in PLA leave the PLA carrying the load. PLA specks in PETG put weak islands in a material bought for its layer bond.

What the documented tests show

In a 2023 Bambu Lab forum test, PETG support for PLA worked at 280 mm³ (PLA→PETG) and 346 mm³ (PETG→PLA). The reverse pair, at 346 and 480 mm³, produced a PETG part that crumbled by hand. Later MakerWorld profiles use 600–800 mm³ for the switch back into the model. One PETG-with-PLA profile keeps the flush into PLA minimal and maxes out PLA→PETG.

Why won’t PETG stick to a PLA interface?

Usually because the PLA surface is too cool and too small for the incoming PETG to wet before it freezes. In a March–April 2026 Snapmaker forum thread, U1 owners reported first PETG layers printing as loose threads at Top Z distance 0. Small areas also gripped poorly, even at 270 °C. Their fixes:

PETG stringing over a PLA support interface during a 3D print.
  • Iron the PLA interface: about 15% failures on small areas without smoothing, 0% with it.
  • Give the first PETG layers their own profile: one user printed them at 280 °C and 4 mm³/s.
  • Keep heat in: the U1 has no heated chamber, so users fit a lid.
  • Start from Snapmaker’s tested values: PLA interface at 230 °C and a 65 °C bed for PETG parts.
Procurement implicationFor PETG parts, write the PLA→PETG flush or the tool-changer route into the job sheet.
Mistake to avoidCopying a PETG-on-PLA profile and simply swapping the two filaments.
How to verifyBars across the PLA→PETG switch must reach your agreed share of solid PETG strength; we use 80%.

3. Support Interface Material Matrix: PLA, PETG, TPU and PA-CF With PVA and HIPS

Choose the interface by the model material, thermal conditions and the printer’s validated material-pair matrix. For the Snapmaker U1 combinations cited here, PETG is the release interface for PLA; PLA is the release interface for PETG and TPU grades of 90A and harder; and a PA/PET breakaway grade is the preferred route for PA-CF. HIPS is used with compatible ABS or ASA systems. PVA or BVOH is appropriate when the support must dissolve in water, subject to grade-specific compatibility.

Which materials don’t bond together in 3D printing?

Snapmaker’s U1 classification marks pairs as strong bonding (+) or bondable (–), meaning weak adhesion that suits dissimilar-material supports. In its U1 matrix, PLA is weak against PETG, TPU, PET, ABS, ASA and PA, while PETG bonds strongly with TPU, PET, ABS, ASA and PC. It uses Snapmaker’s own filaments, with TPU validated at 90A and harder.

Pairing matrix for eight common model–interface pairs

Table 1 turns that screen into a purchasing decision for the pairs B2B buyers ask about most.

On mobile, swipe horizontally to review every column.

Table 1. Support interface pairing matrix (0.4 mm nozzle; sources checked November 2026)
Option (model ← interface)Best use caseKey specAdvantageRiskHow to verifyWhen to rejectSSSray sourcing note
PLA ← PETGPLA housings with flat supported facesTop Z 0 mm; 2–3 layers; flush back to PLA 400 mm³ (our test passed 300)1.6 MPa bond; smooth undersidePETG blobs in the PLA; wet PETG shifts the bondPeel coupon; ISO 527 bar across the switchPETG still strings after 65 °C / 8 h dryingWe ship both spools on one order, batch ID on each label
PETG ← PLAPETG brackets with flat overhangsFlush PLA→PETG 800 mm³ (our test passed 600); PLA ≈230 °C; bed ≈65 °CClean release from PETGPLA residue weakens PETG; first layer stringsBar across the PLA→PETG switch; 7 mm islandLoad path crosses the interface on one nozzleBoth lots quoted and re-tested as one pair
TPU (≥90A) ← PLAGrips and gaskets on tool changersPLA–TPU “bondable” (weak)Rigid support, then peelsOoze from the parked TPU toolPeel coupon; supported-face dimensionsBelow 90A on unvalidated hardwareTPU 95A and PLA in one sample kit
TPU ← PETGBonded rigid–flex overmolds onlyPETG–TPU strong bonding (+)Strong co-printed bondSupport welds to the partNot needed for support useAlways, as a breakaway interfaceSold as an overmold pair, not a support pair
PLA ← PVAInternal channels and cavitiesPrusa MMU profiles: PVA+/BVOH ≈4 mm³/s vs PLA 15 mm³/sDissolves where tools cannot reachMoisture; slow interfaceDissolution test after 24 h exposureNo dry storage at the user sitePVA from 50 spools; see the PVA storage guide
PETG ← PVA or BVOHSoluble support in PETG partsBambu recommends its PVA for PETG; Prusa recommends BVOHSoluble support on PETGGrade-dependent adhesionPair coupon on your PETG lotNo PETG pairing dataWe test PVA against the PETG lot you buy
ABS/ASA ← HIPSABS and ASA housingsd-limonene removalLess moisture-sensitive than PVAOn PETG, one user found HIPS bonded “a little too strong”Dissolution time; interface finishUsed on PETG without a peel testHIPS in 40+ colors for ABS/ASA lines, MOQ from 50 spools
PA-CF / PAHT-CF ← PA/PET breakawayHeated-chamber fixturesPAHT-CF: 260–290 °C nozzle, 80–100 °C bed, 45–60 °C chamberSurvives chamber heatIdle-nozzle heat-ageing; dry 80 °C, 8–12 hCoupon at production chamber temperaturePLA or PETG interface on an 80–100 °C bedPA-CF grades through our custom engineering program

In our pairing matrix, row 4 (PETG with TPU) is a bonded rigid–flex combination, not a breakaway support pair. For PA-CF, row 8 is the heat-resistant PA/PET breakaway route we recommend qualifying at the production chamber temperature.

Pair qualification request: send your printer, nozzle size, model material and the interface you want to test. We review the B2B request, then confirm available grades and sample combination. Standard sample preparation is typically 3–5 working days; freight and applicable documents are confirmed before dispatch. Request a matched pair sample.

What is the best support interface for PLA?

For breakaway work, PETG is a practical commodity option for PLA parts: the cited study measured low tensile strength for its standard PLA/PETG joint, and our own release profile qualifies the pair by lot. Purpose-made grades cost more; Bambu lists its Support for PLA/PETG at US$34.99 per 0.5 kg spool in its US store. PVA or BVOH is useful when a support must dissolve or mechanical removal is unsuitable; see our soluble support filament buyer’s guide.

4. Settings That Make PETG Support for PLA Release Cleanly in OrcaSlicer and Bambu Studio

Assign the second material to the support interface only, then set Top Z distance and interface-layer count for the specific printer and material pair. Our Snapmaker U1 starting profile uses 0 mm Top Z and three solid interface layers; keep both materials dry and verify the first interface layers before production.

What top Z distance for different material supports?

Top Z 0 mm creates direct contact between the interface and the model; it is a starting point, not a universal setting for every printer or filament. The OrcaSlicer documentation describes 0 mm in the context of soluble supports and direct-contact interfaces. For dissimilar breakaway pairs, confirm the slicer behavior and run a small coupon first. In one U1 user test, a purpose-made breakaway PLA interface performed better at 0.1 mm.

OrcaSlicer support interface settings, step by step

  1. Under Filament for supports, set Support/raft interface to the second material and Support/raft base to the model material.
  2. Set Top Z distance 0 mm, 3 top interface layers (2 saves a swap), interface spacing 0 mm and a Rectilinear Interlaced pattern.
  3. Add bottom interface layers, so supports standing on the model also land on the second material.
  4. Use about 0.5 mm XY distance and 2 mm base pattern spacing (Bambu forum recipe); with tree supports, keep support material out of the base (Bambu Lab tip).

Starting print settings by interface pair

Table 2 gathers starting values by pair from manufacturer data sheets, Snapmaker’s guide, dated user tests and our release profile.

On mobile, swipe horizontally to review every column.

Table 2. Starting print settings by interface pair (0.4 mm nozzle, 0.2 mm layers; U1-specific values are identified separately)
ParameterPLA part ← PETG interfacePETG part ← PLA interfaceTPU part (≥90A) ← PLA interfaceBasis
Interface setupU1 starting profile: Top Z 0 mm; 3 interface layers; spacing 0. Other printers: validate Top Z and layer count on a coupon.U1 starting profile: Top Z 0 mm; 3 interface layers; spacing 0; iron where supported. Other printers: validate on a coupon.U1 matrix starting point: Top Z 0 mm; 2–3 layers; verify grade-specific release and bed adhesion.Snapmaker U1 guide; lot trials
Nozzle temperatureU1 profile: PLA 230 °C; PETG 265 °C; PETG max volumetric speed 10 mm³/s. Other printers: use each grade TDSU1 profile: PLA interface 230 °C; PETG model temperature per its grade profilePLA per TDS; TPU per its own TDS and tool profileSnapmaker U1 guide; grade TDS
Bed temperatureU1 PLA-model/PETG-support route: 65 °C shared bed; 35–45 °C applies only to the relevant PLA-only profileU1 PETG-model/PLA-interface route: 65 °CUse the selected TPU grade TDS; confirm bed adhesion separatelySnapmaker U1 guide; Bambu TDS
EnclosureFor mixed PLA/PETG on U1, use the guide’s external-circulation mode. The 50 °C figure is the Top Cover’s maximum internal-circulation condition, not the mixed-print chamber settingFor mixed PETG/PLA on U1, use external circulation; do not assume the 50 °C internal mode is active during the mixed printUse the circulation mode and enclosure conditions specified for the TPU gradeU1 Top Cover; U1 guide; grade TDS
DryingPETG HF: 65 °C × 8 h per grade TDS; do not transfer the setting to every PETG formulationPETG HF: 65 °C × 8 h; Bambu PLA Basic TDS V3.0: 50 °C × 8 hPLA and TPU: follow the exact grade TDS; do not reuse another brand’s drying profileBambu PLA Basic TDS V3.0; Bambu PETG HF TDS V1.0
Nozzle materialStandard (non-abrasive)Standard (non-abrasive)Standard; TPU on its own toolSnapmaker U1 FAQ
Speed rangeInterface at or below model speedFirst PETG layers slow (one user: 4 mm³/s)Slow TPUSnapmaker forum; our release profile
Flush on one nozzleInto PETG ≈280; back 400 mm³ (passed at 300)Into PLA low; back 800 mm³ (passed at 600)Prefer a tool changerBambu forum tests; record SIP-03
Common failurePETG blob in the PLA undersidePETG strings; weak layers aboveTPU strings across the PLAForum reports
FixDry PETG; raise flush back to PLAIron; hotter, slower first layersDry TPU; limit parked-tool oozeForum reports

Change one variable at a time and rerun the same coupon, so each result points to one cause.

Procurement implicationLock slicer build and profile to approved lots; Bambu Studio 2.8.0 changed PLA↔PETG auto-flush.
Mistake to avoidLoading PETG under a PLA or “support” preset, so it prints at the wrong temperature.
How to verifyCheck the preview: interface material, flush volume and nozzle temperature at the first swap.

5. Tool Changer vs AMS: What a Multi-Material Support Interface Costs in Purge

On a single-nozzle printer, each interface layer can require two material changes and roughly 0.8–2.0 g of purge under the settings compared in Table 3. A tool changer can reduce nozzle-flush waste to milligram-scale; the actual job still depends on the tool-change system, priming routine, wiper and purge collection.

Purge scales with the number of layers that contain interface, not with support size. Three interface layers under four overhangs at different heights means 12 interface layers, or 24 swaps on one nozzle.

How much purge between PLA and PETG?

On a single-nozzle AMS, plan 600–800 mm³ for the switch back into PETG, and 400 mm³ or more back into PLA once a lot test confirms it. The Bambu Studio 2.8.0 public beta (June 25, 2026) raised auto-calculated flushing between official material types such as PLA and PETG. Prusa’s MMU guidance for soluble supports sets a floor of 200–240 mm³ instead of the 140 mm³ default.

Table 3 converts those volumes into grams per interface layer, using 1.24 g/cm³ for PLA and 1.27 g/cm³ for PETG (Prusament TDS, ISO 1183).

On mobile, swipe horizontally to review every column.

Table 3. Purge and non-part material per support interface layer (two material changes; shared-nozzle rows are purge-only calculations)
System and settingHow the swap worksPurge / measured waste per changePer interface layer (g)Per 100 layers (g)Tower or wiper accounting
One nozzle + AMS, 800 / 800 mm³Flush through one nozzle800 mm³ each way2.01201Prime tower excluded from calculation
One nozzle + AMS, 280 / 800 mm³Same280 into PETG, 800 back1.35135Prime tower excluded from calculation
One nozzle + AMS, 280 / 400 mm³SameSSSray released PLA-part profile0.8585Prime tower excluded from calculation
One nozzle + AMS, 280 / 346 mm³SameLowest reported working flush setting in the cited test0.7878Prime tower excluded from calculation
Prusa CORE One+ INDX · published referencePassive tool swap≈13 mg per change (Prusa published figure)0.0262.6Wiper; no prime tower in the cited configuration
Prusa CORE One+ INDX · SSSray PLA ↔ PLADedicated tool swap11.6 mg per change; 1,500 logged changes0.02322.32SSSray TC-500 coupon; wiper waste included in measured total
Prusa CORE One+ INDX · SSSray ASA ↔ ASADedicated tool swap13.8 mg per change; 1,500 logged changes0.02762.76SSSray TC-500 coupon; wiper waste included in measured total
Snapmaker U1 · SSSray PLA ↔ PLAFour complete toolheads30.4 mg per change; 1,500 logged changes0.06086.08SSSray TC-500 coupon; prime tower included
Snapmaker U1 · SSSray PETG ↔ TPU 95AFour complete toolheads36.2 mg per change; 1,500 logged changes0.07247.24SSSray TC-500 coupon; prime tower included
Bambu Lab H2C · SSSray PLA ↔ PLAVortek hotend swap39.2 mg per change; 1,500 logged changes0.07847.84SSSray TC-500 coupon; prime tower and chute included
Bambu Lab H2C · SSSray PETG ↔ TPU 95AVortek hotend swap44.8 mg per change; 1,500 logged changes0.08968.96SSSray TC-500 coupon; prime tower and chute included
Bambu Lab H3C · SwaptekNine dedicated print toolsManufacturer states a material switch under 6 s; no SSSray waste-mass result published yetNot measuredNot measuredValidate priming and collection waste on the buyer’s profile

The tool-changer rows use SSSray protocol TCP-26-05, a TC-500 coupon and three 500-change runs per material pair. The measured total includes INDX wiper blobs and, for U1/H2C, the prime tower plus H2C chute material. The per-layer figures assume two tool changes per interface layer. These are system baselines for the listed material pairs, not direct PETG ↔ PLA support-pair waste measurements. See the SSSray tool-changer test records.

Figure 2 plots the shared-nozzle purge calculations against the published INDX reference. The SSSray U1, H2C and INDX measured totals are listed separately in Table 3 because their waste accounting includes different tower, chute or wiper components.

Cumulative purge vs. number of support interface layers

Single nozzle 800/800 mm³: 0, 20.1, 40.2, 60.2, 80.3 g at 0, 10, 20, 30, 40 interface layers. Single nozzle 280/800 mm³: 0, 13.5, 27.0, 40.4, 53.9 g. Single nozzle 280/346 mm³: 0, 7.8, 15.7, 23.5, 31.4 g. Prusa INDX: 0, 0.26, 0.52, 0.78, 1.04 g. Purge (g) 0255075100 010203040 Interface layers in the part 80.3 g53.9 g31.4 g1.0 g
One nozzle, 800 / 800 mm³One nozzle, 280 / 800 mm³One nozzle, 280 / 346 mm³Prusa INDX, ≈13 mg per swap
Figure 2. Shared-nozzle curves are calculated from Table 3 using PLA 1.24 g/cm³ and PETG 1.27 g/cm³; they exclude prime towers. The INDX line uses Prusa’s published ≈13 mg per change. SSSray’s U1, H2C and INDX measured totals, with the listed waste components included, appear in Table 3.

At 40 interface layers, the 800/800 mm³ single-nozzle calculation reaches about 80.4 g. SSSray’s measured PLA ↔ PLA tool-changer baselines calculate to about 0.93 g on INDX, 2.43 g on U1 and 3.14 g on H2C over the same two-change-per-layer assumption. These tool-changer figures are system baselines, not direct PETG ↔ PLA support-pair measurements.

Why tool changers still need a prime or wipe step for support materials

A parked tool is not a frozen tool. Siraya Tech says its PET and PPA breakaway grades need a purge tower on independent-nozzle printers, as All3DP reported. The reason is heat-ageing in the idle nozzle. Tom’s Hardware found an H2C print without its prime tower failed before halfway. Prusa says fast nozzle cooling eliminates oozing from parked INDX tools, and a silicone wiper replaces the wipe tower.

Procurement implicationBudget interface jobs by interface layers × purge per swap, not by part weight.
Mistake to avoidCutting AMS flush to save grams and losing the part to weak layers.
How to verifyWeigh purge and tower from one real job against the slicer estimate.

6. Support Interface Filament Claims vs Reality

Treat every “breakaway”, “zero purge” or “works with any PLA” claim as something to qualify. Performance depends on the printer, material lot and supported geometry. Table 4 shows the document or test we ask a supplier to provide.

On mobile, swipe horizontally to review every column.

Table 4. Support interface filament claims and how to verify them
Vague marketing claimWhat it might hideDocument, sample or test to requestWhat a reliable supplier provides
“Works with all PLA and PETG”Tested on one brand’s lotPeel coupon on your model-material lotNamed lots, printer and slicer build
“Zero purge”Prime tower and wiper blobs not countedGrams of purge and tower from your fileMass per swap or per plate, with conditions
“Tool-free removal”Tested on large flat overhangs onlyRemoval on an island under 10 mmFailure rate on a small-feature coupon
“Dry, vacuum sealed”No moisture valueMoisture result and method on the COAKarl Fischer moisture per batch

A supplier who answers with batch IDs and test records sells a process, not a spool. Compare answers with the filament supplier comparison tool.

7. Multi-Material Support Programs: Four B2B Buyer Scenarios

Qualify the pair against the failure mode that matters in your operation: returns for distributors, first-print complaints for OEM brands, scrap for print farms and interface strength for engineering buyers.

Distributor

Situation: tool-changer customers ask for “support filament”.

Bad choice: generic PETG with no settings, then fused interfaces and returns.

Better choice and check: a PLA + PETG release kit with a settings card and matched batch IDs, peel-tested on two printers.

Request a matched pair sample

OEM Brand

Situation: a starter pack bundled with a four-tool printer.

Bad choice: PETG shipped with only a PLA profile, then stringing and support tickets.

Better choice and check: one profile per pair, tested with as-shipped spools on the bundle printer.

Plan a release kit under OEM/ODM

Print Farm

Situation: 20 tool changers print PLA enclosures with flat undersides.

Bad choice: PETG left open for weeks, then a drifting bond and sanded parts.

Better choice and check: PETG dried 65 °C × 8 h, sealed storage, lots locked to the profile, a peel coupon per lot.

Quote bulk PETG and bulk PLA as one pair

Engineering Buyer

Situation: PETG or PA-CF fixtures with supported datum faces.

Bad choice: PLA on PETG at default flush, or on PA-CF, then weak layers or softened supports.

Better choice and check: a tool changer, ISO 527 bars across the switch and a PA/PET breakaway grade for PA-CF.

Scope an engineering pair

8. SSSray Interface-Pair Release Data: Batch Records, Equipment and Results

We qualify an interface pair like a production lot: both spools, one printer, one locked profile and an auditable record. The October 2026 release below covers one PLA, one PETG and one TPU 95A lot, tested as three pairs.

The SSSray interface-pair dataset (SSSRAY-SIP-2026-10-R01) and thermal qualification dataset (SSSRAY-SIP-THERMAL-2026-11-R01) are published under the Creative Commons Attribution 4.0 International (CC BY 4.0) license. Reuse requires appropriate credit to SSSray, a link to the license and an indication of changes.

Protocol ID: SSSRAY-SIP-2026-10-R01 · Release window: 12–27 October 2026 · Lots: SSR-PLA-261008-L2-B07, SSR-PETG-261009-L3-B04, SSR-TPU95A-260930-L1-B02 · Printers: Snapmaker U1 (tool changer), Bambu Lab P1S + AMS (single nozzle) · Lab atmosphere: 23 ± 2 °C, 50 ± 10% RH (ISO 291)

Release records, October 2026

Table 5 lists the eight records behind the released pairs, with a public benchmark beside each gate where one exists.

On mobile, swipe horizontally to review every column.

Table 5. SSSray interface-pair release records, SSSRAY-SIP-2026-10-R01 (1.75 mm lots; tensile values in MPa, mean of n)
Record IDDateBatch / lotEquipmentMethod / standardSamples (n)ConditionsPass gatePublic benchmarkResult
SIP-01 Moisture2026-10-12PLA-B07, PETG-B04, TPU95A-B02KF-01 tube-oven coulometric Karl Fischer, 180 °CISO 15512:2019 Method B13 per lotAfter drying, before vacuum sealingPLA ≤0.020%; PETG ≤0.025%; TPU ≤0.020%PETG HF TDS: dry 65 °C × 8 hPLA 0.012%; PETG 0.017%; TPU 0.015% (wt%); recorded values below internal numerical gates
SIP-02 Diameter and ovality2026-10-12Same three lotsLM-01 inline laser micrometer, 500 scans/sStart, middle, end of 10 spools30 per lot1.75 mm nominal±0.03 mm; ovality ≤0.020 mm (TPU ≤0.025)—Max deviation 0.018 / 0.021 / 0.024 mm; max ovality 0.011 / 0.013 / 0.017 mm. Pass
SIP-03 Flush ladder2026-10-15PLA-B07 + PETG-B04Bambu Lab P1S + AMS; UTM-01 5 kNFlush back at 200, 300, 400, 600, 800 mm³; legacy Type 1A geometry (ISO 527-2:2012 reference), switch at mid-thickness3 bars per step3 interface layers; slicer build lockedLowest step ≥80% of the solid bar346 passed, 480 failed (2023)Back to PLA: 78 / 88 / 92 / 95 / 96% → 300 mm³. Back to PETG: 52 / 61 / 72 / 84 / 91% → 600 mm³
SIP-04 Release force2026-10-19All three pairsUTM-01, 90° peel fixture, 100 mm/minMethod SIP-M2, 40 × 40 mm coupon5 per pairSnapmaker U1; peeled 24 h after printingHand release, no residue; N/mm reported—PLA←PETG 0.21 ± 0.05; PETG←PLA 0.34 ± 0.07; TPU←PLA 0.29 ± 0.06 N/mm; 15 / 15 clean. Pass
SIP-05 Small islands2026-10-20PETG-B04 part on PLA-B07 interfaceSnapmaker U17 mm island, first model layer on interface10 islands × 3 printsIroned vs not ironed30 / 30 bonded≈15% vs 0% failures (U1 user, 2026)Not ironed 26 / 30 (13% failed); ironed 30 / 30. Pass with ironing
SIP-06 Strength across switch2026-10-22PLA-B07; PETG-B04UTM-01 5 kN, 5 mm/minlegacy Type 1A geometry (ISO 527-2:2012 reference), XY, switch at mid-thickness5 per routeConditioned ≥48 h at 23 °C / 50% RH≥80% of the solid bar1.6 MPa butt joint vs 50 MPa PLA (2025)Solid PLA 50.6, PETG 43.4. PLA on U1 49.4 (98%); PLA at 400 mm³ 47.3 (93%); PETG at 800 mm³ 39.6 (91%). Pass
SIP-07 Supported-face finish2026-10-23PLA-B07 + PETG-B04PRF-01 contact profilometer, λc 0.8 mmISO 21920-2, Ra and Rz3 coupons × 3 tracesVs PLA-on-PLA support at 0.2 mm top ZRa below the control—PETG interface Ra 2.4 µm, Rz 14.8 µm; control Ra 11.6 µm, Rz 63.0 µm. Pass
SIP-08 Parked-tool dwell2026-10-26; retest 10-27All three lotsSnapmaker U1Park 10 min at standby, resume on a test wall10 parks per toolPreset standby temperatures10 / 10 without blob or gapIdle-nozzle heat-ageing (Siraya Tech)PLA 10 / 10; PETG 10 / 10; TPU 9 / 10, then 10 / 10 at standby −20 °C. Pass after change

SIP-01 records KF-01 tube-oven vaporization followed by coulometric Karl Fischer water determination under ISO 15512:2019 Method B1. ISO describes a 0.01 wt% detection limit for Method B and notes that the stated limit depends on the maximum possible test-portion mass. Our recorded 0.012–0.017 wt% results are close to that method limit. The 12 October 2026 release record does not state the historical test-portion mass, so we do not assign a sample mass retrospectively or claim ±0.001 wt% accuracy. The method-specific limit of quantification and measurement uncertainty still require verification for the KF-01 setup.

For the next KF-01 method-verification runs, our proposed target test portion is 1.50 g per determination. At the recorded 120–170 ppm moisture range, that mass would contain approximately 180–255 μg of water. Metrohm’s 899 Coulometer manual advises that a coulometric test portion should contain at least 50 μg of water and lists 1 g as a guide at 100 ppm. This manufacturer guidance supports the proposed test-portion calculation; it does not establish the LOQ or measurement uncertainty of SSSray’s KF-01 method.

As an external equipment reference only, Metrohm Application Note K-049 describes polycarbonate pellet testing with an 885 Compact Oven Sample Changer and 899 Coulometer: approximately 3 g of sample, 250 °C, 50 mL/min nitrogen, n = 10, a mean of 766.7 μg/g and 0.55% RSD. That is Metrohm’s published PC application, not equipment or test data from SSSray and not a validated temperature recipe for PLA, PETG or TPU. The 180 °C value in our SIP-01 table remains the recorded internal KF-01 oven set point. Before treating it as a validated production method, verify complete water release without polymer degradation for each grade, and document blanks, recovery, repeatability, method LOQ and measurement uncertainty.

The released configuration reflects two changes from the initial trials: small islands needed an ironed interface, and the TPU tool needed a lower standby temperature. We report the moisture readings with the method limits and the distinction between historical records and future verification settings.

What the records show

The flush back into PLA passed at 300 mm³, so we release the pair at 400 mm³ for margin. PETG parts passed at 600 mm³, so we release at 800 mm³. At 280 mm³ into PETG and 400 mm³ back, one interface layer purges about 0.85 g on a single nozzle, 58% less than 800/800 mm³. On the U1, PLA kept 98% of its solid strength across the switch. The PETG interface measured Ra 2.4 µm versus 11.6 µm for the PLA-on-PLA control, a 79% lower Ra in these two tested configurations. Because the control used a 0.2 mm top Z distance while the PETG interface used 0 mm, the comparison does not isolate material alone.

PLA and PETG filament spools beside a tensile-test specimen mounted in a testing machine.

Gate sources: moisture, diameter and ovality are assessed against our batch QC benchmarks. SIP-03 and SIP-06 use legacy Type 1A specimen geometry recorded against ISO 527-2:2012; they are SSSray comparative FFF tests, not claims of conformity to the current ISO 527-2:2025 edition. Ask for record SSSRAY-SIP-2026-10-R01, with raw readings and photos, alongside your quote.

Thermal, Annealing and Dimensional Qualification

Protocol ID: SSSRAY-SIP-THERMAL-2026-11-R01 · Qualification window: 1–7 November 2026 · Lots: SSR-PLA-261101-L1-A01, SSR-PETG-261101-L1-B01, SSR-TPU95A-261101-L1-C01 · Printers: Snapmaker U1 · Lab atmosphere: 23 ± 2 °C, 50 ± 10% RH (ISO 291)

This qualification block connects material identity, printed specimen preparation, thermal transitions, post-anneal dimensional stability and a stiffness screen for the three grades in the interface-pair program. We publish individual readings alongside the reported means and ranges so buyers can trace the calculations and compare each result with the stated SSSray release gates.

Qualification record ID: SSSRAY-SIP-THERMAL-2026-11-R01 · Release window: 1–7 November 2026 · Test records: SSSRAY-HDT-2026-11-R01, SSSRAY-VIC-2026-11-R01, SSSRAY-DSC-2026-11-R01, SSSRAY-ANL-2026-11-R01 and SSSRAY-CAN-2026-11-R01.

On mobile, swipe horizontally to review every column.

Qualification lot register and equipment traceability
MaterialLot IDSpecimen preparationPrint profileEquipment / instrument IDDrying and conditioning
PLASSR-PLA-261101-L1-A01FFF bars, 80 × 10 × 4 mm for HDT; 10 × 10 × 4 mm for Vicat; 120 × 10 × 4 mm for cantilever; 0.4 mm nozzle; 0.2 mm layers; 4 perimeters; 100% infill; XY flat orientation210 °C nozzle / 60 °C bed; 60 mm/s; 100% part coolingPRN-01 Snapmaker U1; HVT-01 HDT/Vicat frame; DSC-01 DSC; OV-01 oven; DIM-01 micrometer; CAN-01 cantilever fixture55 °C × 6 h; condition 48 h at 23 ± 2 °C / 50 ± 10% RH
PETGSSR-PETG-261101-L1-B01FFF bars, 80 × 10 × 4 mm for HDT; 10 × 10 × 4 mm for Vicat; 120 × 10 × 4 mm for cantilever; 0.4 mm nozzle; 0.2 mm layers; 4 perimeters; 100% infill; XY flat orientation245 °C nozzle / 75 °C bed; 50 mm/s; 40% part coolingSame instrument set; HVT-01, DSC-01 and OV-01 calibrated against their most recent verification certificate65 °C × 8 h; condition 48 h at 23 ± 2 °C / 50 ± 10% RH
TPU 95ASSR-TPU95A-261101-L1-C01FFF bars, 80 × 10 × 4 mm for HDT; 10 × 10 × 4 mm for Vicat; 120 × 10 × 4 mm for cantilever; 0.4 mm nozzle; 0.2 mm layers; 4 perimeters; 100% infill; XY flat orientation225 °C nozzle / 45 °C bed; 30 mm/s; 50% part coolingSame instrument set; displacement range extended for flexible specimens55 °C × 8 h; condition 48 h at 23 ± 2 °C / 50 ± 10% RH

Printed-specimen geometry follows the ISO test-bar dimensions where applicable; FFF process preparation is declared separately from the ISO test method and is reported for reproducibility, not as an accreditation claim.

Thermal results at a glance

Qualification summary — mean (range); HDT values are 0.45 MPa / 1.80 MPa, Vicat values are A50 / B50
MaterialHDT as-printedHDT post-annealVicat as-printedDSC resultDimensional change mean (range)Cantilever deflection and residual mean (range)
PLA0.45: 61.80 (61.50–62.10) °C
1.80: 54.40 (54.10–54.70) °C
0.45: 92.10 (91.80–92.40) °C
1.80: 72.18 (71.80–72.50) °C
A50: 61.78 (61.50–62.00) °C
B50: 58.10 (57.80–58.40) °C
Xc 18.96 (18.92–19.03)% → 32.87 (32.80–33.01)%ΔX -0.42% (-0.46% to -0.39%); ΔY -0.45% (-0.45% to -0.45%); ΔZ +0.25% (+0.25% to +0.25%); bow 0.32 mm (0.29–0.36)deflection 0.50 (0.48–0.52) mm; residual 0.02 (0.01–0.02) mm
PETG0.45: 72.96 (72.60–73.40) °C
1.80: 66.24 (65.90–66.60) °C
0.45: 73.20 (73.00–73.40) °C
1.80: 66.40 (66.20–66.60) °C
A50: 80.24 (80.00–80.50) °C
B50: 77.40 (77.10–77.70) °C
Tg 80.00 (79.80–80.20) °C; no resolved Tcc/TmΔX -0.07% (-0.07% to -0.06%); ΔY -0.08% (-0.10% to -0.05%); ΔZ +0.25% (+0.25% to +0.25%); bow 0.09 mm (0.08–0.11)deflection 0.83 (0.81–0.86) mm; residual 0.03 (0.03–0.04) mm
TPU 95A0.45: 50.10 (49.80–50.40) °C
1.80: 41.86 (41.50–42.10) °C
0.45: 50.22 (50.00–50.50) °C
1.80: 41.98 (41.70–42.20) °C
A50: 74.72 (74.20–75.10) °C
B50: 27.76 (27.10–28.30) °C
Tg -26.10 (-26.40–-25.80) °C; Tm 176.50 (176.20–176.80) °CΔX -0.02% (-0.02% to -0.01%); ΔY -0.05% (-0.10% to +0.00%); ΔZ +0.25% (+0.25% to +0.25%); bow 0.13 mm (0.11–0.15)deflection 31.86 (30.80–33.10) mm; residual 0.64 (0.50–0.80) mm

Qualification acceptance gates

These limits are the internal release gates declared for this qualification block, so each value can be read against a clear pass/fail criterion. They are SSSray product-release criteria for these grades, not universal polymer specifications, and must not be copied to a different grade or supplier.

Qualification acceptance gates — SSSray release criteria for these three grades
MaterialAs-printed HDT minimum
0.45 / 1.80 MPa
Vicat minimum
A50 / B50
DSC targetPost-anneal dimensional gateCantilever gateResult
PLA≥60 / ≥52 °C
61.80 / 54.40 °C
≥60 / ≥56 °C
61.78 / 58.10 °C
Post-anneal Xc 30–35%
32.87%
|ΔX|, |ΔY| ≤0.60%; |ΔZ| ≤0.50%; bow ≤0.50 mm
Max XY 0.46%; bow 0.36 mm
0.35–0.65 mm; residual ≤0.05 mm
0.50 / 0.02 mm
Pass
PETG≥70 / ≥63 °C
72.96 / 66.24 °C
≥78 / ≥75 °C
80.24 / 77.40 °C
No resolved Tcc/Tm peak in the stated scan
No resolved peak
|ΔX|, |ΔY| ≤0.15%; |ΔZ| ≤0.50%; bow ≤0.20 mm
Max XY 0.10%; bow 0.11 mm
0.65–1.05 mm; residual ≤0.05 mm
0.83 / 0.03 mm
Pass
TPU 95A≥45 / ≥38 °C
50.10 / 41.86 °C
≥70 / ≥25 °C
74.72 / 27.76 °C
Tg −30 to −22 °C; Tm 170–182 °C
−26.10 / 176.50 °C
|ΔX|, |ΔY| ≤0.15%; |ΔZ| ≤0.50%; bow ≤0.20 mm
Max XY 0.10%; bow 0.15 mm
25–40 mm; residual ≤1.00 mm
31.86 / 0.64 mm
Pass

HDT: 0.45 MPa and 1.80 MPa

HDT uses ISO 75-1:2020 with ISO 75-2:2013: Method B at 0.45 MPa and Method A at 1.80 MPa, three-point bending, 64 ± 1 mm support span, 80 ± 2 × 10 ± 0.2 × 4 ± 0.2 mm specimens and a 120 ± 10 °C/h temperature rise. Five separate specimens were used for each material, stress level and condition. Method A and Method B use separate specimens; the annealed and as-printed groups are also independent specimen sets. HDT is a comparative result under the stated stress and geometry, not a universal service-temperature rating.

Record SSSRAY-HDT-2026-11-R01 — individual HDT readings (°C), n = 5 for each stress and condition
MaterialLot IDConditionMethod B · 0.45 MPa
Separate specimen IDs / individual / mean / range
Method A · 1.80 MPa
Separate specimen IDs / individual / mean / range
PLASSR-PLA-261101-L1-A01As-printedPLA-AP-B-01 to -05
61.5 / 61.7 / 61.9 / 62.1 / 61.8
mean 61.8; range 61.5–62.1
PLA-AP-A-01 to -05
54.1 / 54.4 / 54.7 / 54.3 / 54.5
mean 54.4; range 54.1–54.7
PLASSR-PLA-261101-L1-A01Post-annealPLA-AN-B-01 to -05
91.8 / 92.0 / 92.2 / 92.4 / 92.1
mean 92.1; range 91.8–92.4
PLA-AN-A-01 to -05
71.8 / 72.1 / 72.3 / 72.5 / 72.2
mean 72.2; range 71.8–72.5
PETGSSR-PETG-261101-L1-B01As-printedPETG-AP-B-01 to -05
72.6 / 72.9 / 73.1 / 73.4 / 72.8
mean 73.0; range 72.6–73.4
PETG-AP-A-01 to -05
65.9 / 66.2 / 66.6 / 66.4 / 66.1
mean 66.2; range 65.9–66.6
PETGSSR-PETG-261101-L1-B01Post-annealPETG-AN-B-01 to -05
73.0 / 73.2 / 73.4 / 73.1 / 73.3
mean 73.2; range 73.0–73.4
PETG-AN-A-01 to -05
66.2 / 66.5 / 66.6 / 66.3 / 66.4
mean 66.4; range 66.2–66.6
TPU 95ASSR-TPU95A-261101-L1-C01As-printedTPU-AP-B-01 to -05
49.8 / 50.1 / 50.4 / 50.0 / 50.2
mean 50.1; range 49.8–50.4
TPU-AP-A-01 to -05
41.5 / 41.9 / 42.1 / 41.8 / 42.0
mean 41.9; range 41.5–42.1
TPU 95ASSR-TPU95A-261101-L1-C01Post-annealTPU-AN-B-01 to -05
50.0 / 50.3 / 50.5 / 50.2 / 50.1
mean 50.2; range 50.0–50.5
TPU-AN-A-01 to -05
41.7 / 42.0 / 42.2 / 42.1 / 41.9
mean 42.0; range 41.7–42.2

Vicat softening temperature

Vicat follows ISO 306:2022 using 10 × 10 × 4 mm printed coupons; the FFF specimen route is declared separately. A50 applies 10 N at 50 °C/h; B50 applies 50 N at 50 °C/h. Separate specimens are used for each method. The larger B50 load produces a lower result for the flexible TPU 95A grade; do not compare A50 and B50 as if they were the same test method.

Record SSSRAY-VIC-2026-11-R01 — individual Vicat readings (°C), n = 5 for each method and lot
MaterialLot IDISO 306 A50 · 10 N / 50 °C·h⁻¹
Separate specimen IDs / individual / mean / range
ISO 306 B50 · 50 N / 50 °C·h⁻¹
Separate specimen IDs / individual / mean / range
PLASSR-PLA-261101-L1-A01PLA-VIC-A50-01 to -05
61.5 / 61.8 / 62.0 / 61.7 / 61.9
mean 61.8; range 61.5–62.0
PLA-VIC-B50-01 to -05
57.8 / 58.1 / 58.4 / 58.0 / 58.2
mean 58.1; range 57.8–58.4
PETGSSR-PETG-261101-L1-B01PETG-VIC-A50-01 to -05
80.0 / 80.4 / 80.2 / 80.5 / 80.1
mean 80.2; range 80.0–80.5
PETG-VIC-B50-01 to -05
77.1 / 77.4 / 77.7 / 77.3 / 77.5
mean 77.4; range 77.1–77.7
TPU 95ASSR-TPU95A-261101-L1-C01TPU-VIC-A50-01 to -05
74.2 / 74.8 / 75.1 / 74.6 / 74.9
mean 74.7; range 74.2–75.1
TPU-VIC-B50-01 to -05
27.1 / 28.0 / 27.6 / 28.3 / 27.8
mean 27.8; range 27.1–28.3

DSC: Tg, crystallization and melting

DSC uses ISO 11357-1:2023, ISO 11357-2:2020 for Tg and ISO 11357-3:2025 for melting/crystallization. Each run uses a 6 ± 1 mg sample, nitrogen at 50 mL/min and 10 K/min heating/cooling. Tg is reported from the second heating; cold-crystallization and melting enthalpies are reported from the first heating to preserve the specimen’s prior thermal history. ΔHcc is shown as the positive magnitude of the cold-crystallization exotherm. PETG shows no resolved cold-crystallization or melting peak in this scan. TPU crystallinity is not calculated because no grade-specific 100%-crystalline reference enthalpy is assigned.

Record SSSRAY-DSC-2026-11-R01 — individual DSC readings, n = 3 per material and state
MaterialLot IDState / specimen IDsTg (°C)Tcc / Tc (°C)Tm peak (°C)ΔHcc / ΔHc (J/g)ΔHm (J/g)Calculated Xc
PLASSR-PLA-261101-L1-A01As-printed
PLA-DSC-AP-01 to -03
61.6 / 61.9 / 61.8
mean 61.8; range 61.6–61.9
118.7 / 119.3 / 119.0
mean 119.0; range 118.7–119.3
169.1 / 169.5 / 169.3
mean 169.3; range 169.1–169.5
17.8 / 18.2 / 18.0
mean 18.0; range 17.8–18.2
35.4 / 35.9 / 35.6
mean 35.6; range 35.4–35.9
18.92 / 19.03 / 18.92
mean 18.96%; range 18.92–19.03%
PLASSR-PLA-261101-L1-A01Post-anneal
PLA-DSC-AN-01 to -03
62.0 / 62.2 / 62.1
mean 62.1; range 62.0–62.2
109.5 / 110.1 / 109.8
mean 109.8; range 109.5–110.1
169.5 / 169.8 / 169.6
mean 169.6; range 169.5–169.8
8.5 / 8.8 / 8.7
mean 8.7; range 8.5–8.8
39.0 / 39.5 / 39.2
mean 39.2; range 39.0–39.5
32.80 / 33.01 / 32.80
mean 32.87%; range 32.80–33.01%
PETGSSR-PETG-261101-L1-B01As-printed
PETG-DSC-AP-01 to -03
79.8 / 80.2 / 80.0
mean 80.0; range 79.8–80.2
Not resolvedNot resolvedNot resolvedNot resolvedNot resolved
PETGSSR-PETG-261101-L1-B01Post-anneal
PETG-DSC-AN-01 to -03
79.9 / 80.3 / 80.1
mean 80.1; range 79.9–80.3
Not resolvedNot resolvedNot resolvedNot resolvedNot resolved
TPU 95ASSR-TPU95A-261101-L1-C01As-printed
TPU-DSC-AP-01 to -03
-26.4 / -25.8 / -26.1
mean -26.1; range -26.4–-25.8
117.8 / 118.4 / 118.1
mean 118.1; range 117.8–118.4
176.2 / 176.8 / 176.5
mean 176.5; range 176.2–176.8
16.1 / 16.4 / 16.2
mean 16.2; range 16.1–16.4
24.1 / 24.5 / 24.3
mean 24.3; range 24.1–24.5
Not calculated
TPU 95ASSR-TPU95A-261101-L1-C01Post-anneal
TPU-DSC-AN-01 to -03
-26.2 / -25.9 / -26.0
mean -26.0; range -26.2–-25.9
118.0 / 118.2 / 118.1
mean 118.1; range 118.0–118.2
176.3 / 176.7 / 176.6
mean 176.5; range 176.3–176.7
15.8 / 16.1 / 16.0
mean 16.0; range 15.8–16.1
24.4 / 24.7 / 24.5
mean 24.5; range 24.4–24.7
Not calculated

For PLA only, Xc = (ΔHm − ΔHcc) / 93 J·g⁻¹ × 100. The 93 J/g reference enthalpy is a declared calculation assumption for unfilled PLA, consistent with the published PLA DSC crystallinity convention; it is not applied to PETG or TPU. The PLA result rises from 18.96% to 32.87% after the defined anneal, alongside a lower cold-crystallization enthalpy and higher melting enthalpy.

Annealing and dimensional change

Annealing is a declared SSSray method, not an ISO 75 or ISO 306 requirement. PLA: 110 °C × 20 min in a flat restraint, then cool at 1 °C/min. PETG: 70 °C × 30 min, then cool in the fixture. TPU 95A: 50 °C × 120 min, then cool at room temperature. Dimensions are measured before and after treatment on 100 × 20 × 4 mm coupons, with each measurement state conditioned for 24 h at 23 ± 2 °C / 50 ± 10% RH. Δ% = (after − before) / before × 100. Five coupons per lot are reported.

Record SSSRAY-ANL-2026-11-R01 — individual dimensional readings before → after annealing (mm; change in %)
MaterialLot IDSpecimen IDX length
before → after / ΔX
Y width
before → after / ΔY
Z thickness
before → after / ΔZ
Maximum bow after anneal (mm)
PLASSR-PLA-261101-L1-A01PLA-DIM-01100.02 → 99.58
-0.44%
20.01 → 19.92
-0.45%
4.01 → 4.02
0.25%
0.32
PLASSR-PLA-261101-L1-A01PLA-DIM-02100.01 → 99.61
-0.40%
20.00 → 19.91
-0.45%
4.00 → 4.01
0.25%
0.36
PLASSR-PLA-261101-L1-A01PLA-DIM-03100.03 → 99.57
-0.46%
19.99 → 19.90
-0.45%
4.02 → 4.03
0.25%
0.29
PLASSR-PLA-261101-L1-A01PLA-DIM-0499.99 → 99.60
-0.39%
20.02 → 19.93
-0.45%
4.00 → 4.01
0.25%
0.34
PLASSR-PLA-261101-L1-A01PLA-DIM-05100.00 → 99.59
-0.41%
20.00 → 19.91
-0.45%
4.01 → 4.02
0.25%
0.31
PETGSSR-PETG-261101-L1-B01PETG-DIM-01100.01 → 99.94
-0.07%
20.00 → 19.98
-0.10%
4.00 → 4.01
0.25%
0.08
PETGSSR-PETG-261101-L1-B01PETG-DIM-02100.02 → 99.95
-0.07%
20.01 → 19.99
-0.10%
4.01 → 4.02
0.25%
0.11
PETGSSR-PETG-261101-L1-B01PETG-DIM-03100.00 → 99.94
-0.06%
20.02 → 20.00
-0.10%
4.02 → 4.03
0.25%
0.09
PETGSSR-PETG-261101-L1-B01PETG-DIM-04100.03 → 99.96
-0.07%
19.99 → 19.98
-0.05%
4.00 → 4.01
0.25%
0.10
PETGSSR-PETG-261101-L1-B01PETG-DIM-0599.99 → 99.93
-0.06%
20.00 → 19.99
-0.05%
4.01 → 4.02
0.25%
0.08
TPU 95ASSR-TPU95A-261101-L1-C01TPU-DIM-01100.00 → 99.98
-0.02%
20.00 → 19.99
-0.05%
4.00 → 4.01
0.25%
0.12
TPU 95ASSR-TPU95A-261101-L1-C01TPU-DIM-02100.02 → 100.00
-0.02%
20.01 → 20.00
-0.05%
4.01 → 4.02
0.25%
0.14
TPU 95ASSR-TPU95A-261101-L1-C01TPU-DIM-0399.99 → 99.98
-0.01%
19.99 → 19.99
0.00%
4.00 → 4.01
0.25%
0.13
TPU 95ASSR-TPU95A-261101-L1-C01TPU-DIM-04100.01 → 99.99
-0.02%
20.02 → 20.00
-0.10%
4.02 → 4.03
0.25%
0.11
TPU 95ASSR-TPU95A-261101-L1-C01TPU-DIM-05100.03 → 100.01
-0.02%
20.00 → 19.99
-0.05%
4.01 → 4.02
0.25%
0.15

Cantilever screening

Internal SSSray method SSSRAY-CAN-01: 120 × 10 × 4 mm XY-printed bar, 80 mm free span, 0.49 N tip load, 60 s loaded dwell, followed by 60 s unloaded recovery. Deflection is a comparative screening value for this exact geometry and load, not an ISO flexural modulus. TPU undergoes large deflection, so small-deflection beam equations must not be applied to its result.

Record SSSRAY-CAN-2026-11-R01 — cantilever deflection and 60 s recovery readings, n = 5 per lot
MaterialLot IDSpecimen IDTip load (N)Deflection at 60 s (mm)Residual deflection 60 s after unloading (mm)
PLASSR-PLA-261101-L1-A01PLA-CAN-010.490.490.02
PLASSR-PLA-261101-L1-A01PLA-CAN-020.490.510.02
PLASSR-PLA-261101-L1-A01PLA-CAN-030.490.480.01
PLASSR-PLA-261101-L1-A01PLA-CAN-040.490.520.02
PLASSR-PLA-261101-L1-A01PLA-CAN-050.490.500.02
PETGSSR-PETG-261101-L1-B01PETG-CAN-010.490.810.03
PETGSSR-PETG-261101-L1-B01PETG-CAN-020.490.840.04
PETGSSR-PETG-261101-L1-B01PETG-CAN-030.490.820.03
PETGSSR-PETG-261101-L1-B01PETG-CAN-040.490.860.04
PETGSSR-PETG-261101-L1-B01PETG-CAN-050.490.830.03
TPU 95ASSR-TPU95A-261101-L1-C01TPU-CAN-010.4931.200.60
TPU 95ASSR-TPU95A-261101-L1-C01TPU-CAN-020.4932.500.70
TPU 95ASSR-TPU95A-261101-L1-C01TPU-CAN-030.4930.800.50
TPU 95ASSR-TPU95A-261101-L1-C01TPU-CAN-040.4933.100.80
TPU 95ASSR-TPU95A-261101-L1-C01TPU-CAN-050.4931.700.60

Using these qualification results: the individual readings allow buyers to trace the reported means, ranges and PLA crystallinity calculation, compare as-printed and post-anneal HDT, and assess dimensional change and cantilever deflection against their application limits. The lot IDs and test record IDs are SSSray release identifiers; quote them when requesting the corresponding COA or qualification record.

Send us

Printer, nozzle size and slicer build.

Model material and interface: PETG, PLA, PVA or HIPS.

An STL or photo of your hardest supported island.

Monthly spools per SKU, destination and documents needed.

You get back

After review, confirmation of available grades and up to three 1 kg sample spools for qualified B2B evaluation; standard preparation is typically 3–5 working days.

Applicable COA, TDS and SDS confirmed by material and project before dispatch.

Standard samples in 3–5 working days; freight confirmed first.

Qualification orders from 50 spools, in 1 kg, 3 kg or 5 kg spools.

9. PETG Support for PLA FAQ for B2B Buyers

Can you use PLA as support for PETG?

Yes, but treat it as the harder direction of the pair. PLA releases cleanly from PETG, yet PLA residue left in the nozzle weakens the PETG layers printed above it. In a 2023 test, a PETG part with PLA supports crumbled at a 480 mm³ PLA→PETG flush. In our October 2026 flush ladder, PETG bars kept 72% of solid strength at 400 mm³ and 84% at 600 mm³. We therefore release at 800 mm³. On a tool changer, contamination largely disappears, but the first PETG layer can still string, so iron the interface and slow those layers.

Can I use PVA with PETG?

Sometimes, and only after a test on your exact PETG lot. Bambu Lab recommends its PVA for all PLA and PETG, while Prusa’s knowledge base says that for PETG you can practically only use BVOH. Adhesion depends on each formulation, so test the pair rather than the label. In Prusa MMU profiles, PVA+ and BVOH run at about 4 mm³/s versus 15 mm³/s for PLA; both soluble grades must also stay dry. If pliers can reach the support, a PLA breakaway interface is faster and cheaper.

What support material should I use for PA-CF?

Use a purpose-made PA/PET breakaway interface or a soluble grade validated for nylon. Bambu’s PAHT-CF data sheet lists a 260–290 °C nozzle, an 80–100 °C bed and a 45–60 °C chamber. It names Support for PA/PET as the support material. PLA and PETG interfaces soften there, because their heat deflection sits around 55–70 °C at 0.45 MPa. Community users have also reported ASA working as a PAHT-CF interface. Dry both materials first; Bambu specifies 80 °C for 8–12 hours.

Should a distributor stock dedicated support filament or sell PETG support for PLA as a pair?

For most catalogs, sell PETG support for PLA as a documented pair and keep one dedicated support grade for buyers who want zero setup. The pair uses two fast-moving SKUs you already stock, while a dedicated grade moves slowly. Bambu’s Support for PLA/PETG lists at US$34.99 per 0.5 kg spool. What makes the pair sellable is information: a settings card, matched batch IDs and a tested printer list. Without them, the cheap shortcut turns into returns.

Will a different PETG lot or brand change how the interface releases?

It can. Release depends on the PETG’s copolymer, additives and moisture, and Snapmaker warns that a damp support material can bond too tightly or not enough. A lot change can also move the best interface temperature. Lock approved lots to the profile, ask for Karl Fischer moisture on each COA, and rerun a peel coupon and a tensile bar on every new lot. That one check protects every job that follows.

Are the thermal and cantilever readings actual SSSray measurements?

Yes. The thermal, Vicat, DSC, annealing, dimensional-change and cantilever tables are SSSray qualification records published under protocol SSSRAY-SIP-THERMAL-2026-11-R01. Their SSR lot IDs and test records are SSSray release data for the interface-pair program. The interface-pair release records remain separately identified as SSSRAY-SIP-2026-10-R01.

What should an RFQ for a support interface pair include?

Name both materials and their roles, plus the printer, nozzle size and slicer build. Add the hardest geometry, such as the smallest supported island, and your acceptance tests, for example a peel coupon and a tensile bar across the switch. List the documents you need: a COA with moisture, a TDS and an SDS. Finish with monthly spools per SKU, spool size and destination, so the quote covers a qualified pair, not two anonymous spools.

10. Conclusion: Buy PETG Support for PLA as a Qualified Pair

PETG support for PLA works when the selected grades and print profile keep interface adhesion low enough for clean removal. The cited study measured 1.6 MPa for its standard PLA/PETG butt joint, while our own release data sets the purge and interface conditions for specific lots. Heat, pressure, moisture, contamination and geometry can change the result.

The decision logic is short. Choose the pair by chemistry and bed temperature: PLA for TPU, a PA/PET breakaway grade for PA-CF. Set Top Z distance to 0 mm with 2–3 interface layers. Spend purge on the switch back into the model, or move the job to a tool changer, where a swap costs milligrams. Then lock lots, moisture and profile together.

Your next step is a two-spool trial on the printer your customers own, with one peel coupon and one tensile bar across the switch.

Send your printer, nozzle and model material; we confirm the sample route, typical 3–5 working-day preparation, freight and applicable documents after review. Prefer paperwork first? Request the TDS, COA and SDS (MSDS) or compare materials across our 3D printer filament supplier range. You can also ask about OEM packaging for a release kit or request a bulk quote with your printer list and monthly volume.

Request a quote or free samples

Tell us the material, color, spool size and monthly volume. An engineer replies within 24 hours on business days.

11. References

  1. Zatloukal J. et al. (2025). Optimizing Interfacial Adhesion and Mechanical Performance of Multimaterial Joints Fabricated by Material Extrusion. Materials 18(16), 3846: joint tensile data.
  2. Snapmaker Wiki: Using a Different Filament for Support (PLA and PETG): U1 settings, moisture warning.
  3. Snapmaker Support: U1 multi-material printing performance and U1 FAQ: bonding matrix.
  4. Bambu Lab Store: Support for PLA/PETG and Support for PA/PET: products, tips, pricing.
  5. Bambu Lab PAHT-CF TDS V3.0, PLA Basic TDS V3.0 and PETG HF TDS V1.0: print and drying data.
  6. Bambu Studio 2.8.0 Public Beta release notes (June 25, 2026): PLA↔PETG flushing.
  7. OrcaSlicer Wiki: Support Advanced: Z distance and interfaces.
  8. Prusa Knowledge Base: Water-soluble materials (PVA/BVOH): pairing, purge, speeds.
  9. Bambu Lab Community Forum: PETG for PLA and PLA for PETG (2023): recipe and flush tests.
  10. Snapmaker Forum: PLA as interface filament for PETG (March–April 2026): U1 user reports.
  11. Tom’s Hardware: Bambu Lab H2C review (January 14, 2026): prime tower test.
  12. Prusa Blog: CORE One INDX orders now open (April 23, 2026): 13 mg per swap.
  13. Bambu Lab: H3C launch (November 3, 2026): nine Swaptek print tools and manufacturer-stated material switching under six seconds.
  14. Snapmaker U1: Using a Different Filament for Support (PLA and PETG): U1-specific temperatures, bed setting, interface layers and spacing.
  15. Snapmaker U1 Top Cover: passive chamber heat retention up to 50 °C; no active chamber heater.
  16. ISO 75-1:2020, ISO 75-2:2013, ISO 306:2022 (current published edition; ISO lists it as “to be revised”), ISO 11357-1:2023, ISO 11357-2:2020, ISO 11357-3:2025 and ISO 291:2008: current published test-method references.
  17. ISO 15512:2019: plastics water-content determination methods, including Method B1 tube-oven vaporization and the stated method detection capability.
  18. Metrohm 899 Coulometer Operating Instructions: manufacturer guidance on the minimum water amount in a coulometric test portion (50 μg) and indicative sample mass at 100 ppm.
  19. Metrohm Application Note K-049: external PC-pellet oven/KF example using an 885 Compact Oven Sample Changer and 899 Coulometer; not SSSray equipment or a direct PLA/PETG/TPU validation.
  20. ISO 527-2:2025: current edition and updated specimen designations; SSSray’s SIP-03/SIP-06 Type 1A records are identified separately as legacy comparative FFF tests.
  21. SSSray B2B sample policy: up to three 1 kg spools for qualified B2B buyers, typically 3–5 working-day preparation, and project-specific freight/document confirmation.
  22. SSSray Tool Changer 3D Printer Presets: protocol SSSRAY-TCP-PRESET-2026-10-R01: TCP-26-05, 9,000 tool changes, material-pair waste readings and tower/wiper accounting.
He Jiang, Senior Researcher at SSSray
He Jiang
Senior Researcher · SSSray · 3D Printing Filament Manufacturing · Jinhua, Zhejiang

He Jiang is a senior researcher at SSSray, a 3D printing filament manufacturer in Jinhua, Zhejiang, China. This guide covers support interface pairing, flush control and lot qualification for B2B distributors, print farms and OEM partners, based on printer-maker documentation, a peer-reviewed interface study and SSSray’s October 2026 interface-pair release records.