PPA-CF vs PA6-CF: When Heat, Humidity and Failure Cost Justify the Upgrade

PPA-CF vs PA6-CF: B2B Decision Summary

By He Jiang · Senior Researcher, SSSray · Published 28 October 2026

Direct answer: choose PPA-CF when a loaded part must keep stiffness and dimensional stability in warm, humid service; keep PA6-CF when impact tolerance, easier processing and lower material cost matter more. In Bambu Lab’s same-lab comparison, PA6-CF lost 34.8% of its XY bending modulus after the stated wet conditioning, while PPA-CF lost 2.4%.

Best PPA-CF caseLoaded brackets, fixtures and datum parts where heat and humidity act together and wet-state stiffness controls tolerance.
Keep PA6-CF whenThe part is dry or impact-loaded: Bambu’s PA6-CF benchmark reports 15.5 kJ/m² Z-direction impact versus 4.3 kJ/m² for its PPA-CF.
Key specificationDry and conditioned modulus, HDT with the test load stated, Tg for the exact grade, Z-direction data, and the conditioning state of every coupon.
Grade warningPPA-CF is not one formula: current published Tg values include 80 °C for Xenia, 85 °C for Bambu Lab and 120 °C for SSSray’s current 15% CF grade.
Procurement ruleBudget by accepted part and field-failure cost, then qualify the exact grade and production lot before a volume PO.

PPA-CF vs PA6-CF in 2026: What B2B Buyers Need to Decide

PPA-CF is an application-specific upgrade, not a universal replacement for PA6-CF. The decision should be driven by wet-state stiffness, service temperature, failure mode, printer capability and cost per accepted part.

That distinction matters because the label “PPA-CF” covers materially different formulations. Bambu Lab publishes a Tg of 85 °C for its PPA-CF, Xenia publishes 80 °C for XECARB PPA-CF, and SSSray’s current 15% CF PPA-CF grade publishes 120 °C. HDT, drying and print windows also vary by grade. A buyer therefore needs the exact grade TDS and lot-linked qualification record, not a generic PPA family value.

Three purchasing mistakes recur in high-temperature nylon projects: reading HDT without the test load, treating lower moisture absorption as “no drying required,” and selecting the stiffest dry datasheet without checking Z-direction toughness or conditioned performance.

This guide uses four decision tools: a same-lab dry/wet comparison, a Heat–Humidity Upgrade Map, a cost-per-good-part break-even model, and an SSSray evidence block that separates published grade data, first-hand moisture data, a public production-lot QC record and buyer-specific qualification tests.

Key Takeaways for PPA-CF vs PA6-CF Procurement

  • Wet stiffness is the clearest upgrade signal. In Bambu Lab’s same-lab comparison, bending-modulus retention was 65.2% for PA6-CF, 86.1% for PAHT-CF and 97.6% for PPA-CF under the published wet condition.
  • Bambu’s PPA-CF benchmark is roughly 1.8× stiffer dry and 2.7× stiffer wet than its PA6-CF. Bending modulus: 9,860 vs 5,460 MPa dry and 9,620 vs 3,560 MPa wet.
  • PA6-CF still wins on layer toughness in the same benchmark. Z-direction impact is 15.5 kJ/m² for PA6-CF versus 4.3 kJ/m² for PPA-CF.
  • Moisture can move the PA6 matrix into a different mechanical regime. METTLER TOLEDO’s unfilled PA6 study reports Tg around 62 °C dry and about 27 °C near 1% absorbed water at roughly 50% RH.
  • PPA-CF is still hygroscopic. Bambu publishes 1.30% saturated water absorption at 25 °C / 55% RH; SSSray’s first-hand Q1 2026 exposure test measured its tested PPA-CF at 0.50% after 720 h at 23 °C / 50% RH.
  • PPA-CF is grade-specific. Current published Tg values span 80 °C (Xenia), 85 °C (Bambu Lab) and 120 °C (SSSray current 15% CF grade).
  • HDT claims need the load and specimen state. Bambu publishes 227 °C at 0.45 MPa and 196 °C at 1.8 MPa for its PPA-CF; SSSray publishes 214 °C at 0.455 MPa and 176 °C at 1.82 MPa for its current grade.
  • The October 2026 Bambu retail snapshot is about 2.5× apart per kilogram. PPA-CF is $149.99 per 0.75 kg (about $200/kg) and PA6-CF is $79.99 per 1 kg. This is a dated US retail reference, not an SSSray quotation.
  • In the worked 120 g bracket model, the upgrade breaks even near a 10% PA6-CF field-failure rate. Replace the model inputs with your own material price, yield, machine cost and failure cost before approving a PO.

1. PPA-CF vs PA6-CF: What Actually Changes in the Part

The dominant change is the polymer matrix, but carbon-fiber loading and the rest of the formulation also vary by grade. PPA is a semi-aromatic polyamide; PA6 is aliphatic. The aromatic content can raise stiffness and thermal stability and usually reduces moisture sensitivity, but the exact result belongs to the exact commercial grade.

At the molecular level, water plasticises polyamides by increasing chain mobility. PPA’s semi-aromatic structure restricts that mobility more than PA6, which is why a well-formulated PPA-CF can retain far more stiffness after conditioning. That mechanism does not make every PPA-CF grade equivalent.

Why PA6-CF loses a third of its stiffness in humid air

Water acts as a plasticiser in nylon. METTLER TOLEDO’s DMA work on unfilled PA6 reports a dry Tg of about 62 °C and roughly 27 °C at about 1% absorbed water near 50% RH; the conditioning series ran for about 200 hours to approach equilibrium at the stated atmospheres.

For a printed PA6-CF fixture, the practical consequence is not a fixed number of days but a change in stiffness and creep as the part approaches its service-moisture equilibrium. Wall thickness, coating, airflow and temperature all change the rate, so procurement specifications should define the conditioning state rather than assume a “dry” datasheet remains representative in service.

PPA is a family, not one polymer

“PPA” covers several semi-aromatic chemistries and compounded filament systems. Current filament examples make the spread obvious: Xenia XECARB PPA-CF publishes Tg 80 °C, Bambu Lab PPA-CF 85 °C, and SSSray’s current 15% CF PPA-CF grade 120 °C. Those values should not be merged into one “PPA Tg.”

That matters because HDT, Tg, crystallinity, fiber content and print orientation answer different engineering questions. For a purchasing file, record the exact grade revision and request DSC or other lot-level confirmation when Tg is a design-critical acceptance point.

Table 1 lines up one lab’s dry and wet data, so the comparison is apples to apples. Values come from the same specimen geometry and conditioning, which is rare in filament marketing.

On mobile, swipe horizontally to review every column.

Table 1. Same-lab dry vs wet properties: PA6-CF, PAHT-CF and PPA-CF (Bambu Lab published data, checked October 2026)
Property (XY unless noted)Bambu PA6-CFBambu PAHT-CFBambu PPA-CFTest condition
Bending modulus, dry5,460 MPa4,230 MPa9,860 MPa80 × 10 × 4 mm, 100% concentric infill
Bending modulus, wet3,560 MPa3,640 MPa≈9,620 MPa (−2.4%)Saturated at 25 °C / 55% RH
Bending strength, dry → wet151 → 95 MPa125 → 115 MPa208 → 202 MPaSame specimens
Saturated water absorption2.35%0.88%1.30%25 °C / 55% RH
HDT, 0.45 MPa186 °C194 °C227 °CISO 75, dry state
HDT, 1.8 MPa164 °CNot published196 °CISO 75, not annealed
Impact strength, Z15.5 kJ/m²13.3 kJ/m²4.3 kJ/m²ISO 179, dry
Tensile strength102 MPa92 MPa168 MPaISO 527

Read Table 1 in two directions. Across the rows, PPA-CF wins every stiffness and heat line; down the last rows, PA6-CF keeps a large lead in layer toughness.

Bending stiffness retained after moisture saturation (higher = more stable)

Figure 1. Wet bending modulus ÷ dry bending modulus, calculated from Bambu Lab’s published parameter comparison (wet = saturated at 25 °C / 55% RH; 80 × 10 × 4 mm specimens). Scale 0–100%.

The gap between 65% and 98% is the whole upgrade argument. If your drawing was approved on dry PA6-CF numbers, a humid installation quietly removes a third of the stiffness you designed around.

2. The Heat–Humidity Upgrade Map: When PPA-CF vs PA6-CF Becomes a Clear Call

Direct answer: PPA-CF becomes the stronger candidate when heat, humidity and sustained load act on the same part. Heat alone or humidity alone does not automatically justify the upgrade.

Our screening map uses three questions: will the part spend long enough in service to approach its moisture equilibrium, is the service temperature high enough for matrix softening or creep to matter, and does the failure mode favor stiffness or impact tolerance? The thresholds below are SSSray engineering screening rules derived from the cited grade data; the production part still has to pass its own load, creep and conditioning test.

Rule 1: humidity decides whether dry data applies

If the part will remain around 50% RH or higher long enough to approach equilibrium, design with conditioned data rather than assuming the dry TDS. METTLER’s thin PA6 specimens required roughly 200 hours in the controlled atmospheres used in that study; real printed parts can condition faster or slower depending on thickness, temperature, airflow and coatings.

Rule 2: temperature decides whether the matrix is glassy

Unfilled PA6 in the cited METTLER study moves from about 62 °C Tg dry to roughly 27 °C near 1% absorbed water. PPA-CF grades move that threshold by different amounts: published examples in this guide range from 80–85 °C to 120 °C. Use the exact grade Tg and a creep or heat-soak test at the real service load rather than treating “PPA-CF” as one thermal number.

Rule 3: load type decides whether stiffness or toughness wins

Fixture datums, sensor mounts and precision brackets fail by drift, so stiffness wins. Clips, guards and handling tools fail by cracking, so toughness wins. A part that does both needs a design change, not just a material change.

Table 2 turns the three rules into a material call you can write into a specification.

On mobile, swipe horizontally to review every column.

Table 2. Heat–Humidity Upgrade Map for carbon fiber polyamides (SSSray engineering rules, derived from published Tg, HDT and wet-retention data)
Service conditionLoad typeRecommended materialWhy (published evidence)Verify before PO
Dry indoor (<40% RH or sealed/coated), ≤50 °CImpact, snap, handlingPA6-CFZ impact 15.5 kJ/m² vs 4.3 kJ/m² for PPA-CFDrop test on the printed part
Humid (≥50% RH sustained), ≤50 °CModerate stiffnessPAHT-CFBending strength retained 92%; AMS-compatible feedingWet-conditioned bending coupon
Humid, elevated temperature, sustained loadStiffness or tolerance criticalPPA-CF candidateBambu benchmark retains 97.6% wet modulus; SSSray current grade publishes 130–150 °C continuous-use guidanceExact-grade Tg + conditioned modulus + creep/heat-soak on the part
Any humidity, datum or gauge fixtureDimensional driftPPA-CFDry modulus 9,860 MPa; wet ≈9,620 MPaCMM check after 14 days at shop RH
Beyond the qualified PPA-CF service window, or aggressive chemical exposureStatic load / chemical resistancePPS-CF candidateBambu PPS-CF publishes HDT 235 °C at 1.8 MPa and 0.05% water absorptionZ coupon + chemical soak + any required grade/part-specific flame report

Notice that PPA-CF earns two rows, not all of them. The map is designed to stop over-buying as much as under-buying.

Procurement implicationWrite the service RH and temperature into the RFQ; they decide which datasheet column applies.
Mistake to avoidApproving PA6-CF on dry coupons for a part that will live in a humid plant.
How to verifyCondition coupons to equilibrium, then test bending and dimensions against the drawing.

3. Is PPA-CF Better Than PA6-CF? Where PA6-CF Still Wins

For the benchmark grades compared here, PPA-CF leads on heat, stiffness and humid stability, while PA6-CF leads on toughness, easier processing and price. “Better” depends on how the part fails.

Toughness and layer adhesion

The stiffest filament is not the most forgiving. Bambu’s PPA-CF data shows Z-direction elongation of 0.9% and Z impact of 4.3 kJ/m², while PA6-CF reaches 15.5 kJ/m² in the same direction. A PA6-CF part also gets tougher when damp: XY impact rose from 40.3 to 57.2 kJ/m² in the wet state.

Picture a tote-handling guide that gets bumped by forklifts all day. PA6-CF bends and survives; a PPA-CF version may hold the datum more tightly but fail more abruptly along a layer line under one severe impact.

PPA-CF vs PA6-CF impact toughness test specimens in Jinhua

Printability and throughput

Printer demand is grade-specific. Bambu’s PA6-CF baseline is 260–290 °C on an 80–100 °C bed; Bambu’s PPA-CF baseline moves to 280–310 °C and a 100–120 °C bed. SSSray’s current PPA-CF page lists 260–290 °C as the recommended nozzle range, with 300 °C marked optimal; 70–100 °C as the recommended bed range, with 110 °C marked optimal; and a 50–80 °C chamber recommendation. For the Bambu ecosystem specifically, PA6-CF and PPA-CF are not AMS-compatible, while PAHT-CF is.

Price per kilogram

Our 27 October 2026 US retail snapshot puts Bambu PPA-CF at $149.99 per 0.75 kg and Bambu PA6-CF at $79.99 per 1 kg, roughly a 2.5× gap per kilogram. That comparison is useful for the worked model because it holds the brand constant; it is not a wholesale market average and it is not an SSSray quotation.

Price note: the figures in this article are dated US retail references used for calculation, not a guaranteed market average. SSSray provides volume-specific factory pricing and will quote competitively against the required grade, quantity, packaging, documents, Incoterm and destination.

Procurement implicationKeep PA6-CF as the default SKU; add PPA-CF as an application-approved upgrade, not a replacement.
Mistake to avoidSwitching a whole fixture library to PPA-CF because one part failed in heat.
How to verifyPrint the same part in both materials and run the real failure mode: drop, clamp cycle or heat soak.

4. PPA-CF vs PA6-CF Cost per Good Part: When the Upgrade Pays

Direct answer: the upgrade pays when PA6-CF parts fail in service often enough that replacement cost outweighs the PPA-CF material premium. In our model, the break-even is about a 10% field failure rate.

The formula is short: cost per good part = (material + machine time + labour) ÷ print yield + field failure rate × cost of one field failure. Material is rarely the biggest number; a failed bracket on a running line almost always is.

Scenario A — US Branded-Retail Benchmark: a 120 g Sensor Bracket

This is an illustrative procurement model, not measured SSSray field-failure data. Inputs: 120 g part; PA6-CF at $80/kg and PPA-CF at $200/kg from the dated Bambu retail snapshot above; 5 machine-hours at $3/h; $6 of labour and drying; print yield 94% for PA6-CF and 92% for PPA-CF; $180 per field failure for replacement, downtime and shipping; PPA-CF field failures held at 1%.

Scenario A: cost per good part vs PA6-CF field failure rate (120 g bracket)

PA6-CF: 0% failure $32.55, 5% $41.55, 10% $50.55, 15% $59.55, 20% $68.55. PPA-CF with 1% field failure: $50.71 at every point. The lines cross at about 10%. $ per good part $20$35$50$65$80 0%5%10%15%20% PA6-CF field failure rate $32.55$68.55 $50.71
PA6-CF ($80/kg, 94% print yield)PPA-CF ($200/kg, 92% yield, 1% field failure)
Figure 2. Scenario A uses the dated Bambu US retail benchmark: (material + $15 machine time + $6 labour) ÷ yield + failure rate × $180.

Below about 10% field failures, PA6-CF is cheaper per good part; above it, PPA-CF wins and keeps winning. If a failure costs $500 instead of $180, the same model moves the break-even to about 4.3%.

Procurement implicationApprove the upgrade from field failure data, not from the datasheet comparison alone.
Mistake to avoidComparing price per kg when the part weighs 120 g and a line stop costs hundreds.
How to verifyLog 60–90 days of PA6-CF field returns by root cause; only heat or humidity failures count toward the upgrade.

5. PPA-CF vs PAHT-CF vs PPS-CF: Choosing the Right High-Temperature Carbon Fiber Filament

PAHT-CF is a lower-moisture bridge for many moderate-heat nylon jobs, PPA-CF is the stronger candidate when conditioned stiffness and heat act together, and PPS-CF becomes relevant when the qualified PPA-CF service window or chemical resistance is not enough. None of those transitions should be made from a material name alone.

2026 PPA-CF grades worth knowing

Xenia’s XECARB PPA-CF uses a bio-based PPA with 52% renewable content and 20% carbon fiber; the currently served official TDS reports Tg 80 °C and HDT 235 °C at 0.45 MPa and 205 °C at 1.80 MPa. Antinsky’s PPA-CF30HT launch data, reported by 3DPrint.com, states 30% carbon fiber, 12,136 MPa flexural modulus and 176 °C HDT, but the article does not state the HDT load. That is exactly why the load must stay attached to an HDT number.

PPA-CF vs PPS-CF

Bambu PPS-CF publishes 0.05% water absorption and 235 °C HDT at 1.8 MPa. Its TDS also describes flame-retardant / self-extinguishing behaviour, but that wording is not a substitute for a grade- and thickness-specific UL 94 report when a project requires a formal flammability classification. The mechanical trade-off is severe Z-direction toughness: Bambu publishes 24 MPa Z tensile and 2.8 kJ/m² Z impact, with a 310–340 °C nozzle window.

Table 3 is the shortlist we would put in front of a purchasing meeting.

On mobile, swipe horizontally to review every column.

Table 3. Carbon and glass fiber polyamide options compared for B2B buyers (published data, checked October 2026)
OptionBest use caseKey specAdvantageRiskHow to verifyWhen to rejectSSSray sourcing note
Bambu PA6-CF benchmarkDry indoor jigs, guards, impact-loaded toolsHDT 186 °C (0.45 MPa); water 2.35%Tough, lowest cost, easier printingLoses ~35% stiffness when wetWet-conditioned bending couponHumid service with tight toleranceDefault engineering SKU; dry-box guidance on label
Bambu PAHT-CF benchmarkHumid shops, moderate-heat nylon parts, Bambu auto-feed workflowsHDT 194 °C (0.45 MPa); water 0.88% (Bambu benchmark)Wet strength retained 92%; Bambu AMS compatibleLower dry stiffness than Bambu PA6-CFDry vs wet modulus from the same labYour conditioned creep or stiffness requirement is not metUseful bridge tier for distributors
Bambu PPA-CF benchmarkHot and humid loaded parts, datum fixturesHDT 196 °C (1.8 MPa); wet modulus −2.4%Stiffness stable wet and warmLow Z impact; ~2.5× retail priceDSC Tg, HDT at 2 loads, Z couponImpact or snap-fit partsMatched PA6-CF/PPA-CF sample pair
High-fiber PPA-CF (30% CF)Ultra-stiff brackets replacing machined partsFlexural modulus 12,136 MPaHighest stiffness per gramNozzle wear; HDT load often unstatedAsk HDT load and Z dataSupplier cannot state HDT loadQualify per part; larger nozzle advised
PPA-GFHeat-resistant parts where carbon-fiber conductivity is undesirableAsk HDT at 1.8 MPa and measured surface resistivityGlass fiber avoids the intrinsic conductivity of carbon fiberFinal compound can still contain conductive additives; still abrasiveResistivity + HDT report on the exact gradeElectrical behavior is assumed from filler name aloneOffered alongside PPA and PPA-CF
PPS-CFHigh heat and aggressive chemical environments beyond the qualified PPA-CF windowHDT 235 °C (1.8 MPa); water 0.05% (Bambu benchmark)Very low moisture uptake and strong chemical resistanceZ impact 2.8 kJ/m²; 310–340 °C nozzleChemical soak + Z coupon + required flame reportPrinter/process or toughness margin is insufficientQuote only after printer capability and compliance scope are confirmed

If two rows look like a fit, pick the cheaper, tougher one and test it first. Moving up a rung is easy; moving down after a failed launch is expensive.

6. PPA-CF vs PA6-CF Printing: Drying, Bed, Chamber and Nozzle Requirements

There is no single PPA-CF print profile. Use the exact commercial grade’s TDS, then lock the production profile on the printer that will make the part.

What printer can print PPA-CF?

A practical qualification printer needs an abrasion-resistant nozzle, enough hotend and bed headroom for the selected grade, stable enclosure temperature and a dryer that can reach the grade’s specified drying cycle. For Bambu PPA-CF, the published window is 280–310 °C nozzle and 100–120 °C bed. SSSray’s current 15% CF grade uses a different window, which is why a generic “PPA profile” is not a purchasing specification.

Is PPA-CF hygroscopic?

Yes. Bambu publishes 1.30% saturated water absorption at 25 °C / 55% RH. SSSray’s Q1 2026 first-hand study measured the tested PPA-CF at 0.12% after 24 h and 0.50% after 720 h at 23 °C / 50% RH, versus 0.55% and 2.40% for the tested PA6-CF. Those are different exposure methods, so use each dataset for its stated condition rather than merging them.

PPA-CF filament drying beside an enclosed 3D printer in Jinhua

Does PPA-CF need annealing?

Not automatically. The Bambu PPA-CF benchmark values cited in this guide are published for the stated test condition without requiring you to assume an annealed part. Annealing can change crystallinity, dimensions and toughness, so if your application uses annealing, qualify the actual post-process and record shrinkage on the drawing-critical dimensions. Our engineering-filament annealing guide covers that qualification route.

Table 4 keeps manufacturer-specific settings separate so a print farm can see the real process load before quoting.

On mobile, swipe horizontally to review every column.

Table 4. Grade-specific starting points for PA6-CF and PPA-CF (verify the current TDS before locking a production profile)
ParameterBambu PA6-CFBambu PPA-CFSSSray PPA-CF 15% CFXenia XECARB PPA-CF
Nozzle temperature260–290 °C280–310 °C260–290 °C recommended; 300 °C marked optimal280–300 °C
Bed temperature80–100 °C100–120 °C with glue70–100 °C recommended; 110 °C marked optimal90–110 °C
Chamber / enclosureEnclosed printerEnclosed; chamber condition affects Z properties50–80 °C recommendedClosed chamber suggested
Drying80 °C, 8–12 h100–140 °C, 8–12 h; keep <20% RH100 °C, 8–12 h; dry before critical printingFollow the current official grade TDS revision before locking the cycle
Nozzle materialHardened / wear-resistantHardened steel mandatory; 0.6 mm recommendedHardened steel or ruby requiredHardened steel; ≥0.4 mm
Published speed guidance<100 mm/s<100 mm/s40–150 mm/sLock by flow and part qualification
Procurement implicationAsk which grade and TDS revision the quote is based on before comparing printer requirements.
Mistake to avoidCopying one brand’s PPA-CF drying or bed setting into another grade’s production SOP.
How to verifyRun a locked-profile full-spool trial, then test Z coupons and drawing-critical dimensions on the production printer.

7. PPA Filament Supplier Claims vs Reality

A PPA-CF claim is only procurement-grade evidence when the test condition, specimen state, grade identity and method stay attached to the number. SSSray uses that same rule for our own grade data and supplier comparisons.

Table 5 converts the six claims we see most often into document requests.

On mobile, swipe horizontally to review every column.

Table 5. Common PPA-CF claims and how to verify them
Vague marketing claimWhat it might hideDocument, sample or test to requestWhat acceptable evidence contains
“HDT up to 235 °C”0.45 MPa load only, or annealed specimensISO 75 report at 0.45 and 1.8 MPaBoth loads, with as-printed or annealed state named
“Moisture-proof PPA”A 24 h ISO 62 value, not saturationSaturated uptake at stated °C and RHUptake plus dry/wet modulus on the same specimen
“High-temperature nylon, Tg 120 °C+”A resin family value, not the filament lotDSC curve at 10 °C/min for the lotLot DSC with Tg, Tm and crystallization peak
“30% CF = strongest”Weak Z adhesion, faster nozzle wearZ tensile and Z impact dataXY and Z values from the same print settings
“Bio-based PPA”Unclear share or basis of renewable contentRenewable content declaration and methodA stated percentage, such as Xenia’s 52%
“Prints on any enclosed printer”TDS printed in a hotter chamber than yoursPrinter, chamber and nozzle used for specimensSpecimen conditions on the TDS

For SSSray PPA-CF projects, we keep the same evidence path on reorders: approved grade revision, lot identity, COA/QC record and any application-specific qualification result. That is more useful than a broad “high quality” claim because the buyer can audit what changed.

8. SSSray First-Hand Data, Public Batch QC and PPA-CF Qualification Controls

Direct answer: SSSray separates grade-level TDS values, first-hand exposure data, public production-lot QC and buyer-specific qualification results so a buyer can see exactly what has already been measured and what will only exist after the quoted lot is tested.

Qualification record: SSSRAY-PPA-PA6-UPG-2026-10-R01 · Revision date: 27 October 2026 · Scope: matched PPA-CF / PA6-CF qualification for 1.75 mm engineering filament · Buyer-lot format: SSR-[material]-[YYMMDD]-L[line]-B[batch]

Dataset use: the SSSray first-party data below is public to read. SSSray retains rights to the dataset; contact SSSray before reuse or republication.

Published SSSray evidence already available before your PO

On mobile, swipe horizontally to review every column.

Table 6A. SSSray published grade data and first-hand control records used in this PPA-CF vs PA6-CF decision
Evidence recordIdentity / batchEquipment / methodSample basisConditionsPublished resultWhat it proves
SSSray PPA-CF released grade dataCurrent 15% CF grade; TDS revision 2026-08; grade-level typicals and spec window; lot reference SSR-PPA-CF-261005-L01-B07ISO 527-2, ISO 178, ISO 75-2, ISO 11357-2, ISO 62 as listed on the current product/TDS recordPer current TDSXY / stated standard conditionsTensile 117 ± 5 MPa; tensile modulus 7,728 MPa; flexural 182 MPa; flexural modulus 7,853 MPa; Tg 120 °C; HDT 214 °C @0.455 MPa and 176 °C @1.82 MPa; 24 h water absorption 0.2–0.4%; Vicat 234 °C; Charpy 7–13 kJ/m²; Tm 310–325 °CDefines the SSSray grade baseline and the release window; the lot reference identifies the release, it does not turn these values into per-coupon lot results
Q1 2026 PA-CF 30-day moisture exposureFour SSSray PA-CF production batches; individual batch IDs were not published in the original studyCalibrated moisture balance; controlled 23 °C / 50% RH exposure; protocol cross-checked against ISO 62:2008n = 3 printed bars per grade; seven time points0.5 mm bars stored open; 0–720 hPPA-CF: <0.10% at 0 h, 0.12% at 24 h, 0.32% at 168 h, 0.50% at 720 h. PA6-CF: <0.10%, 0.55%, 1.55%, 2.40% at the same time pointsFirst-hand SSSray evidence that the tested PPA-CF gained moisture much more slowly than the tested PA6-CF under the same exposure
Public engineering-nylon production-lot QCBatch SSR-PA6-66-260918-L07-B01 · Line 07 · 18 September 2026Continuous inline laser micrometer; 80 °C × 8 h pre-seal conditioning; Karl Fischer titration10 spools × 3 archived laser checkpoints = 30 diameter sets; moisture n = 3Commercial 1.75 mm engineering-nylon lot before packingMean diameter 1.751 mm; observed 1.731–1.772 mm; max ovality 0.018 mm; mean pre-seal moisture 0.017 wt% (170 ppm); lot releasedDemonstrates SSSray’s public lot-to-line traceability and release-control method; it is a QC-control example, not a PPA-CF performance proxy

What SSSray records on the actual PPA-CF / PA6-CF buyer lot

The rows below are the qualification plan for an actual buyer lot. The measured result is attached only after testing; the grade-level values that already exist are listed in Table 6C, and the buyer-lot columns are filled in from the UPG-R01 test rather than forecast in advance.

On mobile, swipe horizontally to review every column.

Table 6B. SSSRAY-PPA-PA6-UPG-2026-10-R01 buyer-lot qualification matrix
TestActual lot identityEquipment / methodSamplesConditionsRelease record
Dry vs conditioned flexural modulusExact PPA-CF and PA6-CF batch IDs from the same qualification windowUniversal tester + climate chamber; ISO 178; conditioning route recordedn = 5 per material per stateDry and conditioned sets; temperature/RH/time written into the recordMean, SD and retention % reported on the buyer qualification file
DSC grade confirmationExact PPA-CF batch IDDSC; ISO 11357-2; heating rate recordedn = 3Dried filamentTg, Tm and Tc attached to the lot record when requested
Z-direction toughnessBoth exact material lotsPendulum impact tester; ISO 179-1n = 5 per materialBuyer printer/profile and chamber state recordedSide-by-side Z result and failure mode photos
Lot releaseEvery quoted production lotInline laser diameter monitoring + lot moisture methodContinuous dimensional monitoring + defined moisture samplePre-seal / after controlled dryingLot COA links the measured values to the batch ID; release limits follow the approved grade specification

Evidence boundary: the Q1 moisture dataset did not publish the four individual PA-CF batch IDs, so we do not present it as lot-specific proof. The public batch SSR-PA6-66-260918-L07-B01 demonstrates the separate SSSray production-lot QC system. Your PPA-CF order receives its own lot identity and result record after qualification.

PPA-CF vs PA6-CF Grade Record: Published Measured Values, Test Methods and the Values Your Lot Must Beat

Record anchor: SSSRAY-PPA-PA6-UPG-2026-10-R01 · Grade reference: SSSray PPA-CF 15% CF, TDS revision 2026-08 · Comparison anchor: published same-lab PA6-CF / PPA-CF conditioned benchmark · PPA-CF lot reference: SSR-PPA-CF-261005-L01-B07 (Line 01, 5 October 2026) · QC-system example: SSR-PA6-66-260918-L07-B01

Table 6C puts four published grade datasets in one frame and keeps the method and specimen state attached to every cell. Where SSSray has not published a conditioned or saturated value, the cell carries the release limit the shipped lot must meet instead of a number without a source. The table therefore reads as a specification: a lot outside those limits is rejected, and its measured value is printed on that lot’s COA.

On mobile, swipe horizontally to review every column.

Table 6C. PPA-CF vs PA6-CF grade data as published, with test method and specimen state attached (release limits marked; checked 27 October 2026)
PropertySSSray PPA-CF 15% CF (value or release limit)Bambu PPA-CFBambu PA6-CFXenia XECARB PPA-CF 20% CFMethod / specimen state
Glass transition temperature, Tg120 °C85 °Cn.p.80 °CDSC, ISO 11357-2, dry filament
HDT at 0.45 MPa214 °C (0.455 MPa)227 °C186 °C235 °CISO 75-2 Method B, dry, as printed
HDT at 1.80 MPa176 °C (1.82 MPa)196 °C164 °C205 °CISO 75-2 Method A, dry, as printed
Vicat softening temperature234 °Cn.p.n.p.n.p.ISO 306 B120, 50 N, 120 °C/h, dry, as printed
Flexural modulus, dry7,853 MPa9,860 MPa5,460 MPan.p.ISO 178, XY, 80 × 10 × 4 mm
Flexural modulus, conditioned≥7,380 MPa (release limit)≈9,620 MPa3,560 MPan.p.SSSray UPG-R01 conditioned release specification; minimum 7,380 MPa, equivalent to ≥94.0% retention against the 7,853 MPa dry-grade reference. The measured buyer-lot value is recorded on the qualification file and lot COA.
Modulus retention after conditioning≥94.0% (release limit)97.6%65.2%n.p.Conditioned mean ÷ dry mean; ≥94.0% is the SSSray UPG-R01 lot-release limit. Bambu’s 97.6% value is shown only as an external same-lab benchmark and is not used to set the SSSray limit.
Flexural strength, dry → conditioned182 MPa208 → 202 MPa151 → 95 MPan.p.ISO 178, same specimens
Tensile strength117 ± 5 MPa168 MPa102 MPan.p.ISO 527-2, XY
Impact strength, ISO 179-1 (orientation as published)7–13 kJ/m² (XY; orientation not stated)4.3 kJ/m²15.5 kJ/m²n.p.ISO 179-1, dry. The SSSray range is the published Charpy value, not a Z-direction result; Bambu values are Z-direction. Z on the SSSray lot is issued under UPG-R01.
Saturated water absorption≤1.4% (release limit)1.30%2.35%n.p.25 °C / 55% RH to saturation; ≤1.4% is the SSSray UPG-R01 lot-release ceiling. It is a separate release specification and is not derived from the 24 h ISO 62 immersion value of 0.2–0.4%.
Water absorption, 24 h0.2–0.4%n.p.n.p.n.p.ISO 62, 24 h immersion
Continuous-use guidance130–150 °Cn.p.n.p.n.p.SSSray grade guidance; confirm by creep test on the part
Print window260–290 °C nozzle (300 optimal); bed 70–100 °C (110 optimal); chamber 50–80 °C280–310 °C; bed 100–120 °C260–290 °C; bed 80–100 °C280–300 °C; bed 90–110 °CGrade TDS; lock the profile on your printer

n.p. = not published for that exact grade in the cited source. release limit = the floor or ceiling applied to a shipped lot under protocol UPG-R01; a lot outside it is rejected and its measured value is printed on the lot COA. SSSray figures come from the current 15% CF TDS revision and product page; Bambu figures come from its published same-lab dry/wet comparison; Xenia figures come from the XECARB PPA-CF TDS accessed 27 October 2026.

Read the last three columns together and the trade-off is fixed: PPA-CF holds stiffness in humid service, PA6-CF absorbs impact energy along the layer lines. A part that needs both is a design problem, not a sourcing problem.

What SSSray can measure, and what lands on your lot file

Protocol SSSRAY-PPA-PA6-UPG-2026-10-R01 defines the measurement set, so the same fields follow every order instead of changing with the salesperson. Table 6D is the capability behind it.

On mobile, swipe horizontally to review every column.

Table 6D. UPG-R01 measurement capability and where each result is produced
MeasurementStandard / methodRange and resolutionExecutionLot file attachment
HDTISO 75-2 Method A and Method B0.45 MPa and 1.80 MPa; RT–300 °CSSSray QC thermal labReport number on the COA when the drawing calls for it
Vicat softening temperatureISO 306 B120, 50 N, 120 °C/hRT–300 °CSSSray QC thermal labOn request, exact grade revision stated
DSC Tg / Tm / TcISO 11357-2, 10 °C/min, nitrogen purge−50–400 °CAccredited partner laboratoryCurve plus peak table on request
Flexural and tensile propertiesISO 178, ISO 527-210 kN frame, 0.001 mm crosshead resolutionSSSray QC lab plus partnerMean, SD and n on request
Z-direction impactISO 179-1, Charpy1 J and 5 J pendulumsSSSray QC lab plus partnerReading set plus failure-mode photos
ConditioningISO 1110 accelerated conditioning70 °C / 62% RHClimate chamberRecorded with every conditioned result
Filament diameter and ovalityIn-line dual-axis laser micrometer0.001 mm resolution, 100% of lengthIn-line on the extrusion lineEvery lot COA
MoistureKarl Fischer titration; ISO 62 gravimetric cross-check10 ppm resolutionSSSray QC labEvery lot COA, pre-seal value
Dimensional checkCMM, ISO 103600.1 µm resolutionSSSray metrologyOn request, drawing datums named
Annealing responseForced-air oven with dummy-specimen thermocoupleUp to 150 °C, loggedSSSray QC labRecorded whenever annealing is specified
Procurement implicationAsk for the UPG-R01 field set, not for a “test report”: the field names are what make two suppliers comparable.
Mistake to avoidAccepting a conditioned modulus figure with no conditioning route and no specimen count.
How to verifyMatch the report number on the COA to the batch ID on the spool label before releasing goods to production.

Scenario B: SSSray factory-cost model for the same 120 g bracket

Scenario A above runs on branded US retail prices. Scenario B runs on factory-level material prices for the same 120 g bracket in warm, humid service, which is closer to a volume order. The yield and field-failure inputs are assumptions in the model, not measured field data; replace them with your own line and service records before approving a PO.

On mobile, swipe horizontally to review every column.

Table 6E. Scenario B cost-per-accepted-part model with stated inputs (120 g bracket, warm/humid service)
Input or controlPPA-CFPA6-CFBasis / calculationResultBuyer interpretation
Material price input$42/kg$24/kgFactory reference for the quoted grade; final price depends on grade, volume, packaging and Incoterm1.75× per kilogramThe gap that dominates a spool-level conversation
Material per part$5.04$2.880.120 kg × $42 vs 0.120 kg × $24$2.16 delta per partThe premium collapses once it is expressed per finished part
Machine time$12$124 h × $3/h on the same printerEqualProcess time is not the differentiator here
Labour and drying$6$510 h dry cycle, setup and spool handling+$1Drying is real but small next to part value
First-pass yield (assumption)93%96%Assumed; replace with your line’s measured yield−3 pointsThe PPA-CF process penalty has to be priced in
Field failure rate (assumption)2%8%Assumed service exposure; replace with 60–90 days of returns data−6 pointsThe single input that can reverse the decision
Cost of one field failure$120$120Replacement part, downtime, shippingHeld constantFailure cost dominates at volume
Cost per accepted part$27.17$30.31PPA: ($5.04 + $12 + $6) ÷ 0.93 + 2% × $120
PA6: ($2.88 + $12 + $5) ÷ 0.96 + 8% × $120
PPA-CF is 10.3% lowerModel output, not a field measurement
PA6-CF break-even failure rate≈5.4% with PPA-CF held at 2%Same inputs, yielding $20.71 base cost for PA6-CFAbove 5.4%, PPA-CF is the lower-cost routeScenario A lands near 10% because its retail price and failure cost differ

The material premium here is $2.16 per part, while one field failure costs $120. That ratio is the entire argument: at roughly 5.4% PA6-CF failures the two routes meet, and every failure above that line is paid for out of margin. Run your own yield, failure rate and downtime cost through the same formula before you sign.

Buyer takeawayIn the same-lab benchmark PPA-CF keeps 97.6% of its dry bending modulus after conditioning against 65.2% for PA6-CF, and Scenario B still returns the lower accepted-part cost at an 8% PA6-CF field-failure rate.
Reject the comparison whenThe supplier cannot attach HDT load, specimen state, conditioning route or lot identity to the reported number.
Qualification routeBefore releasing the drawing, check that the lot report issued under UPG-R01 meets the three release limits in Table 6C, then hold every reorder to the same limits.

For a useful first reply, send service temperature, humidity, load/failure mode, printer and chamber capability, monthly volume, packaging route and destination. SSSray normally returns an initial B2B quotation or clarification within one business day when the project details are complete.

9. B2B Scenarios: Who Should Upgrade from PA6-CF to PPA-CF

Distributor

Situation: customers ask for “the heat-resistant carbon fiber nylon.”

Bad choice: replacing the PA6-CF SKU with PPA-CF across the catalog.

Consequence: price-sensitive buyers leave; impact-loaded parts crack.

Better choice: keep PA6-CF, add PPA-CF with the Upgrade Map on the product page.

Verification: dry/wet data and both HDT loads on every TDS.

Next step: plan a two-tier CF line.

OEM Brand

Situation: launching a private-label PPA-CF in 2026.

Bad choice: printing “HDT 227 °C” on the box with no load.

Consequence: customers design to the wrong number; claims follow.

Better choice: label 0.45 and 1.8 MPa values and the drying window.

Verification: ISO 75 report and lot DSC behind the label.

Next step: set label data under private label.

Print Farm

Situation: quoting brackets for a humid food or packaging plant.

Bad choice: quoting PA6-CF from dry datasheet values.

Consequence: brackets sag within weeks; free reprints erase margin.

Better choice: quote PPA-CF for loaded parts, PA6-CF for guards.

Verification: 14-day humid soak and CMM check on first articles.

Next step: run a production-lot trial.

Engineering Buyer

Situation: a sensor mount near a 90 °C motor in a humid enclosure.

Bad choice: jumping straight to PPS-CF “to be safe.”

Consequence: brittle layers and a 310–340 °C process for no gain.

Better choice: PPA-CF, qualified on wet modulus and Z impact.

Verification: matched-pair coupons under protocol UPG-R01.

Next step: send the drawing for review.

PPA-CF 3D printed sensor mount beside an industrial motor in Jinhua

10. PPA-CF vs PA6-CF FAQ for B2B Buyers

What is PPA-CF filament?

PPA-CF is polyphthalamide filament reinforced with chopped carbon fiber. Commercial grades differ in polymer chemistry, carbon-fiber loading and additives, so the material name is not a complete specification. Current examples in this guide include 15% CF SSSray PPA-CF and 20% CF Xenia XECARB PPA-CF. For procurement, keep the exact grade TDS, Tg, HDT test load, print window and lot identity attached to the quotation.

Is PPA-CF better than PA6-CF?

PPA-CF is the stronger candidate when conditioned stiffness, dimensional stability and heat matter more than impact tolerance and material cost. In Bambu Lab’s same-lab comparison, its PPA-CF retained 97.6% of dry XY bending modulus under the published wet condition versus 65.2% for PA6-CF, while PA6-CF published 15.5 kJ/m² Z-direction impact versus 4.3 kJ/m² for PPA-CF. Choose by the part’s failure mode, not by the material hierarchy.

How hot can PPA-CF parts get?

There is no universal PPA-CF service temperature. Bambu publishes HDT 227 °C at 0.45 MPa and 196 °C at 1.8 MPa for its grade; SSSray’s current 15% CF grade publishes 214 °C at 0.455 MPa, 176 °C at 1.82 MPa and 130–150 °C continuous-use guidance. HDT is not a continuous-use rating, so validate creep, load, orientation and conditioning on the actual part.

Is PPA-CF hygroscopic, and does it need drying?

Yes. Lower moisture uptake does not mean no drying. Bambu publishes 1.30% saturated water absorption at 25 °C / 55% RH and a 100–140 °C, 8–12 h drying cycle for its grade. SSSray’s current PPA-CF grade specifies 100 °C for 8–12 h. Use the exact grade TDS, keep the spool sealed with desiccant, and print critical jobs from controlled dry storage.

What does PPA-CF cost per kg in 2026?

In the 27 October 2026 US retail snapshot used for this article, Bambu PPA-CF is $149.99 per 0.75 kg, about $200/kg, while Bambu PA6-CF is $79.99 per 1 kg. Those are dated brand-retail references, not a universal market average or an SSSray quote. SSSray provides project-specific factory pricing; compare landed cost per accepted part after yield, drying, machine time and field-failure cost.

What should a PPA-CF RFQ include?

State service temperature, humidity, load type, failure mode and printer capability first. Then request the exact grade and fiber content, HDT at the stated load, Tg, dry and conditioned mechanical data, Z-direction properties, drying and storage window, lot COA/QC route, TDS/SDS, required RoHS or REACH documentation, packaging moisture control and written change-notice rules for repeat orders.

Can I test PPA-CF and PA6-CF side by side before ordering?

Yes. Print matched coupons and the real part on the production printer, keep geometry and profile variables controlled, condition one set to the defined service state, and compare stiffness, dimensions and the actual failure mode. SSSray’s UPG-R01 route records the material lot, printer, profile, conditioning state, sample count and result so the approved sample can be checked against the production reorder.

What measured PPA-CF data does SSSray publish before an order?

The current 15% CF TDS revision publishes ISO 527-2 tensile 117 ± 5 MPa, ISO 178 flexural 182 MPa and flexural modulus 7,853 MPa, DSC Tg 120 °C, ISO 75-2 HDT 214 °C at 0.455 MPa and 176 °C at 1.82 MPa, Vicat 234 °C, Charpy impact 7–13 kJ/m², 24 h water absorption 0.2–0.4% and 130–150 °C continuous-use guidance. The Q1 2026 first-hand exposure test measured 0.12% at 24 h and 0.50% at 720 h at 23 °C / 50% RH against 0.55% and 2.40% for the tested PA6-CF. Public lot QC record SSR-PA6-66-260918-L07-B01 documents mean diameter 1.751 mm (1.731–1.772 mm), maximum ovality 0.018 mm and 170 ppm pre-seal moisture. Conditioned modulus, modulus retention and saturated water absorption are controlled by the SSSray UPG-R01 release limits stated in Table 6C; the measured buyer-lot results, together with Z-direction impact and dimensional drift, are recorded on that lot’s qualification report before the drawing is released.

What MOQ, lead time and documents does SSSray offer for PPA-CF?

SSSray’s current PPA-CF page lists neutral packaging from 50 rolls and OEM packaging typically from 500–1,000 rolls. Standard lead time is 7–15 working days and customized orders typically 15–25 working days after specification and packaging confirmation. For each order, SSSray confirms the applicable TDS, SDS/MSDS, RoHS/REACH scope, COA/batch traceability and any project-specific CE or third-party documentation before the PO. Qualified B2B buyers can request up to three complimentary sample spools for evaluation.

11. Conclusion: The PPA-CF vs PA6-CF Decision in One Test

The PPA-CF vs PA6-CF decision comes down to the failure mode and the exact grade. If the part loses tolerance or creeps after moisture and heat act together, PPA-CF can justify its higher material and process cost. If the part fails by impact or lives in a dry, moderate-temperature environment, PA6-CF can remain the better engineering choice.

Use the Heat–Humidity Upgrade Map to shortlist, the cost-per-good-part model to build the business case, and the evidence checklist to keep Tg, HDT load, conditioning state, Z properties and lot identity attached to the approval. If the qualified PPA-CF service window is not enough, screen PPS-CF or another high-temperature material against the actual chemical, thermal and compliance requirement.

The next step is a matched-pair qualification on your production printer: two identified lots, identical coupons and parts, a defined dry/conditioned split, and the real failure-mode test. That gives you an approval record that can be audited again on the reorder.

Prefer to start with paperwork? Request the TDS, COA and MSDS, compare materials across our 3D printer filament supplier range, ask about OEM packaging, or request a bulk quote with your service temperature, humidity and monthly volume.

Request a quote or free samples

Tell us the material, color, spool size and monthly volume. An engineer replies within 24 hours on business days.

12. References and Data Sources

  1. Bambu Lab PPA-CF product data: same-lab dry/wet bending comparison, saturated water absorption, drying and printing settings.
  2. Bambu Lab PA6-CF product data: PA6-CF dry/wet mechanics, Z-direction impact, HDT and PAHT-CF comparison.
  3. Bambu Lab Filament Guide: cross-material mechanical and thermal reference.
  4. Xenia XECARB PPA-CF official TDS: 20% carbon fiber, 52% renewable content, Tg, HDT and print settings; accessed 27 October 2026.
  5. Xenia XECARB PPA-CF product page: material positioning and current product description.
  6. METTLER TOLEDO UserCom 24: Influence of absorbed moisture on Polyamide 6: moisture-conditioning time and Tg shift with absorbed water.
  7. 3DPrint.com, 6 October 2026: manufacturer-supplied Antinsky PPA-CF30HT launch data used only where the article identifies it as such.
  8. SSSray PPA-CF current grade page: 15% CF, mechanical/thermal data, drying, print window, MOQ and lead time.
  9. SSSray TDS/SDS download center: current PPA-CF TDS availability and revision path.
  10. SSSray PA-CF 30-day moisture study: first-hand PPA-CF and PA6-CF exposure data at 23 °C / 50% RH, n = 3 per grade.
  11. SSSray engineering-filament qualification record: public production-lot QC record SSR-PA6-66-260918-L07-B01, inline diameter and Karl Fischer moisture evidence.
  12. ISO 75-2:2013: current confirmed HDT methods for plastics; Method A uses 1.80 MPa and Method B uses 0.45 MPa.
  13. ISO 306:2022: current Vicat softening temperature methods, including B120 at 50 N and 120 °C/h.
  14. ISO 1110:2019: current accelerated conditioning method for polyamide test specimens.
He Jiang, Senior Researcher at SSSray
He Jiang
Senior Researcher · SSSray · 3D Printing Filament Manufacturing · Jinhua, Zhejiang

He Jiang is a senior researcher at SSSray, a 3D printing filament manufacturer in Jinhua, Zhejiang, China. This guide focuses on high-temperature carbon fiber polyamides, comparing PPA-CF, PAHT-CF and PA6-CF through dry and wet property data, lot-level qualification and cost-per-good-part analysis for distributors, print farms, OEM brands and engineering buyers.