PEBA vs TPU for 3D Printed Insoles: B2B Buyer & QC Guide

TL;DR: PEBA vs TPU for Insoles Is a Zoning Decision

For buyers comparing PEBA vs TPU for 3D printed insoles, this is not a winner-takes-all choice. PEBA is the lower-density, rebound-focused option in this comparison at about 1.02 g/cm³. TPU offers broader hardness choices and a lower-cost path for many B2B programs; 64D TPU can hold arch and heel-cup geometry that soft elastomers cannot.

Best optionA zoned insole architecture is the best fit: TPU 64D for the arch shell and heel cup; PEBA 90A where low weight and rebound lead; and foaming TPU 90A where soft cushioning and lower material cost lead.
Poor-fit conditionsPEBA is a poor fit for offloading insoles that need damping more than spring. Foaming TPU is a poor fit when the part must hold a tight density tolerance across many printers.
Key specificationShore hardness of the printed coupon, not just the filament. Density by ISO 1183 or ISO 845. Rebound by a named method such as ASTM D2632.
Supplier evidenceVolume approval should be supported by lot-linked TDS values, a drying specification and coupon hardness at the target infill.
SSSray qualification ruleDrop-test, Bayshore and “energy return” figures use different methods. We do not rank a 70% drop-test claim against a 60% Bayshore result unless the method, specimen and test conditions are the same.

How SSSray Qualifies PEBA vs TPU for Insole Programs

Custom insoles and foot orthotics are a commercially relevant application for flexible filament because the workflow can connect a foot scan, a zoned lattice design and a repeatable print profile. That gives clinics, insole brands and footwear teams a digital alternative to repeated manual trimming and layered-EVA adjustment.

In 2026 the material question changed. PEBA filament moved further into commercial FDM catalogs, with grades now listed by eSUN and Siraya Tech, while TPU stayed the default and active-foaming TPU products such as colorFabb varioShore added another way to cut printed-part density.

Four misconceptions can turn an insole material purchase into an expensive qualification failure. The Shore number on the spool is not the hardness the foot will feel; the highest rebound is not always the right target for pressure redistribution; active foaming changes density with nozzle temperature and flow; and a filament supplier cannot make the finished orthotic device compliant on the buyer’s behalf.

The B2B logic is material selection by zone, lattice selection by load, and lot-level evidence that locks both together. This guide follows the four angles that matter commercially. They are replacing EVA and milled orthotics, getting zoned hardness in one print, prototyping for a single patient, and reducing weight through foaming.

The decisions below separate three evidence layers: peer-reviewed 2025–2026 insole studies, current manufacturer technical data and SSSray lot/qualification records. That makes it possible to distinguish published material properties from printed-part behavior and from the checks a B2B buyer can put into a purchase specification.

Key Takeaways

  • PEBA is the lighter spring. Our PEBA 90A lists 1.02 g/cm³ against 1.2–1.3 g/cm³ for solid TPU. That is roughly 15–22% less mass for the same lattice.
  • Rebound claims need a method. eSUN reports up to 70% for PEBA versus 52% for TPU in its own drop test. Siraya reports 60% Bayshore (ASTM D2632) for foamed PEBA. These are different tests, so direct comparison is valid only when the same method is used.
  • Filament hardness is not insole hardness. A 2026 study printed 60 Shore A TPU as a 20% gyroid and measured 26–65 Shore A across the insole surface.
  • A 14–22% infill window is the supported trial range. An iJOE 2026 study found 22% honeycomb performed best among honeycomb, rectilinear and gyroid patterns.
  • TPU 64D belongs in the shell, not the cushion. Its best fit is arch support and heel cups, where the geometry must hold its shape.
  • Foaming turns temperature into a density dial. In Siraya’s data, foamed PEBA falls from 0.73 to 0.55 g/cm³ between 240 and 270 °C, so a small temperature drift changes the product.
  • EVA is matched on comfort, not yet beaten. Printed and EVA insoles scored 7.5 and 7.8 out of 10 for overall comfort in a five-patient 2026 study.
  • The device maker carries the regulatory file. In the US, intended use and the exact product code determine the route; multiple Class I codes under 21 CFR 890.3475 are 510(k)-exempt, while QMSR/CGMP exemption status must be checked by product code. In the EU, custom-made devices follow MDR Article 52(8) and Annex XIII.
  • Printed-coupon qualification is the relevant acceptance basis. The purchase order should carry lot-to-lot hardness and density tolerances, not only a diameter tolerance.

1. PEBA vs TPU for 3D Printed Insoles: What Actually Differs?

For material selection: both are block copolymers built from hard and soft segments, but they are optimized differently. PEBA’s polyamide and polyether blocks favor low density and elastic energy return. TPU offers a broader commercial hardness range and more damping-oriented formulations, with a lower-cost path for many B2B programs.

The functional difference is spring-led versus damping-led behavior. A performance insert can prioritize elastic energy return, while a pressure-relief orthotic can prioritize energy dissipation. That is why “better” depends on the job the insole has to do.

What is PEBA filament, and why does it spring back faster?

PEBA (polyether block amide, also sold as TPE-A) joins stiff nylon-type segments to soft polyether segments. The nylon blocks act as anchor points, while the polyether chains stretch and recoil with little internal friction. Arkema, which makes Pebax resin, states that its grades can be up to 20% lighter than TPU and COPE and lose less energy than TPU after being stressed.

Our PEBA filament data sheet for the 90A grade lists a density of 1.02 g/cm³, a hardness of 90 Shore A (33 Shore D), a glass transition of −53.7 °C and no-break Izod and Charpy impact. The low glass-transition value supports PEBA’s low-temperature flexibility advantage, but it is not a standalone minimum service-temperature rating.

Why We Start Many Insole Programs with TPU

TPU comes in more hardness steps, from the soft 60A grades used in clinical studies up to semi-rigid 64D. That range makes TPU practical for damping-focused cushion zones, structured shells and top-layer concepts, depending on the specific grade and geometry.

TPU is also the more established FDM route. Printers, slicer profiles and operators already know it, and in SSSray B2B programs it is generally the lower material-cost path than PEBA.

Table 1 puts the published numbers side by side. The source column is critical because several values come from different tests and cannot be ranked directly.

On mobile, swipe horizontally to review every column.

Table 1. Published density, hardness and rebound data for insole elastomers (checked October 2026)
Material (grade)Density, g/cm³Shore hardnessPublished rebound and methodDryingSource and test condition
PEBA 90A, solid1.0290A / 33DNot on TDS; measured per program80 °C, 6–8 hOur PEBA 90A TDS; typical values on printed specimens
PEBA-85A, solid1.0585AUp to 70% vs TPU average 52% (drop test)Not statedeSUN, March 2026; manufacturer’s own drop test
PEBA, foamed (Rebound PEBA Air)0.73 → 0.5581A → 70A60% Bayshore, ASTM D263270–75 °C, 4–6 hSiraya Tech TDS; printed at 240–270 °C; density by ISO 845
TPU, solid (varioShore, unfoamed)1.2–1.395ANot statedNot statedcolorFabb; printed at 190–200 °C (no foaming)
TPU, foamed (varioShore)0.70–0.9095A → 55ANot statedNot statedcolorFabb; printed at 200–250 °C, flow 60–70%
TPU 64DLot TDS required64DNot statedDrying required if popping or bubbles appearOur TPU 64D product data
TPU 90A foamingVaries with temperature90A baseNot stated55–60 °C, 6–8 hOur foaming TPU 90A data; 220–240 °C recommended

In the published examples above, solid PEBA sits about 15–22% below the solid TPU reference in density. Active foaming then creates an even larger density shift, which is why temperature, flow and the test method must stay attached to every comparison.

Density of insole elastomers, solid and foamed (lower = lighter part)

Figure 1. Density in g/cm³, scaled to 1.30 = full bar. Solid values are material densities. Foamed values are printed-part densities (ISO 845 for PEBA Air), so they depend on temperature and flow. Range bars are drawn to the upper bound.

For our buyer qualification, we require density by ISO 1183 (solid) or ISO 845 (printed foam), plus rebound by a named method on printed coupons. We do not treat a quote without a named test method as a usable specification.

2. Can 3D Printed Insoles Replace EVA Insoles and Milled Orthotics?

For production planning: 3D printed insoles can replace major parts of the manual workflow today, but the 2026 evidence supports comparability rather than blanket superiority over EVA. The commercial advantage is repeatable geometry, digital zoning and easier design iteration.

Conventional custom insoles are built like a layered cake. In a 2026 study from Rostock, the EVA layers ran from 20 Shore A on top to 50 Shore A at the base, and a technician fitted each pair by hand. The authors describe the conventional route as plaster casting, manual adjustment and repeated rounds of physical prototyping.

Are 3D printed insoles comfortable? What the 2026 evidence says

  • Rostock, Applied Sciences, April 2026: five patients remained for gait and comfort analysis after one patient was excluded for changing shoes; plantar-pressure analysis was limited to four because Pedar calibration failed for one additional patient. The printed insole used gyroid TPU 60 Shore A at 20% infill and was compared with layered EVA. In the four-patient pressure analysis, walking peak pressure was 197.2 kPa for the printed insole and 172.2 kPa for EVA, both below the 200 kPa threshold cited by the authors. In the five-patient comfort analysis, overall comfort scored 7.5 versus 7.8 out of 10, while forefoot comfort was 5.9 versus 8.1.
  • Systematic review, JOSI, December 2025: six Scopus-indexed studies of FDM TPU and TPE insoles for flatfoot. They reported higher arch height and better comfort, but the review also flagged limited material options and inconsistent print quality.
  • Discover Materials, July 2026: TPU, lightweight TPU and lightweight PLA insoles all reduced maximum plantar pressure compared with barefoot and a wool insole. Comfort and long-term wear were not tested.

Together, these studies show printed insoles holding level with EVA in small trials. The forefoot comfort gap in the Rostock study is the most useful buying signal, because it shows that top-layer softness and edge finish still need work.

Same-Day 3D Printed Orthotic Insoles: What the Current Evidence Supports

Technically, the chain is short. In the Rostock workflow, software sized the insole automatically from the scan, and printing ran at 40 mm/s for infill and 20 mm/s for walls. However, the authors state plainly that they did not compare production time or cost.

We would not publish a “same-day” production claim until a scan-to-fit pilot supports it. For an insole program, we use a ten-pair pilot with failed-print logging and a direct comparison against the current EVA lead time before turning speed into a commercial promise.

What we specifySeparate specifications for the top layer and forefoot zone are justified because that is where printed insoles lost comfort points in 2026 data.
What we rejectMarketing printed insoles as clinically superior to EVA on the current evidence.
How we verifyA timed ten-pair pilot with in-shoe pressure mapping against the current EVA product provides the relevant comparison.

3. PEBA vs TPU Selection by Insole Zone: Which Shore Hardness Goes Where?

Material selection by zone: TPU 64D where the insole must hold its shape, PEBA 90A where low mass and rebound lead, foaming TPU 90A where a lighter and softer cushion is the target, and TPU 85A/90A where damping and material cost lead.

What Shore hardness is best for 3D printed insoles?

There is no single best number, because the lattice changes what the foot feels. In the Rostock study, 60 Shore A TPU printed as a 20% gyroid measured 26–65 Shore A across the insole surface. That was close to the 22–56 Shore A range of the EVA insoles it replaced.

Filament hardness and lattice geometry act together, so the practical starting map is zone-specific:

  • Heel strike zone: PEBA 90A at low infill when rebound and low mass lead, or foaming TPU when softer damping and weight reduction lead.
  • Medial arch and heel cup: TPU 64D or denser TPU 90A, to hold geometry under load.
  • Forefoot: softer, thinner and lower infill, because this is where printed insoles lost comfort points.
  • Top cover: foamed TPU or a textile layer for comfort; any material intended for prolonged skin contact must be qualified separately for that intended use.
PEBA and TPU insole zone lattice selection for heel, arch and forefoot

Zoned hardness in one print: multi-material or single-material?

There are two routes. The multi-material route prints each zone from a different filament. SILIKE’s TCT Asia 2026 post-show recap reports PEAK’s 3D NextFit shoes using multi-hardness TPU zones of 85A and 90A.

The single-material route keeps one filament and varies infill density, wall count and local thickness. The Rostock team did this by varying the height of the insole geometry to change local stiffness.

For B2B programs, single-material zoning is easier to qualify, because there is one lot and one drying spec to control. Multi-material zoning gives a wider range, but it doubles lot control and adds an interface that must not delaminate.

Table 2 summarizes how we match each material option to an insole program, the test we use to confirm it and the condition that stops approval.

On mobile, swipe horizontally to review every column.

Table 2. Insole material options compared for B2B buyers
OptionBest use caseKey specAdvantageRiskHow we verifyRejection triggerSSSray sourcing note
PEBA 90ASports insoles; heel and forefoot rebound lattices; midsole prototypes1.02 g/cm³; 90A / 33D; dry 80 °C, 6–8 hLowest-density solid elastomer in this table; rebound-focused; Tg −53.7 °C supports low-temperature flexibilityHigher material cost; moisture-sensitive; can feel too lively for offloading-focused designsSame-method rebound and compression on printed coupons at your infillNo drying spec, no lot-linked density, or coupon hardness outside toleranceNeutral MOQ 50 spools; 1 kg spools; ±0.03 mm; see PEBA range
TPU 85A / 90AGeneral comfort insoles; top layers; budget programsShore 85A–90A; direct-drive feedingLower cost; damping; wide operator know-howHeavier than PEBA; soft grades buckle in long feed pathsFeed test on the target printer; coupon hardnessFeeding failures that persist after dryingStandard lines: TPU 85A and TPU 90A
TPU 64DArch shells, heel cups, posts and support lattices64D; 225–235 °C nozzleHolds geometry; feeds more easily than soft TPUUsually too firm for comfort as the direct-contact top layer; use a separately qualified comfort layer where requiredArch deflection under load; coupon fatigueCracks at lattice nodes after fatigue testingNeutral MOQ 50 spools; up to 3 sample spools for qualified buyers
TPU 90A foamingLightweight comfort zones; top layers; midsole prototypes220–240 °C; flow reduced as foaming risesDensity and hardness tuned by temperatureDensity can shift across machines or lots when hot-end temperature, flow or moisture are not controlledDensity (ISO 845) on coupons at your locked temperatureDensity shift beyond tolerance at the same profile0.6 mm nozzle helps larger cushions; dry at 55–60 °C
Layered or milled EVA (baseline)Conventional custom insolesLayered 20→50 Shore A (2026 Rostock study)Established clinical workflow and comfortManual, trial-and-error; hard to reproduce a pair exactlyControl baseline for the pressure-mapping pilotBenchmark baselineBenchmark only; we do not supply EVA

For programs qualifying one material first, TPU 64D plus a separately qualified soft top layer covers the widest range of structured orthotic geometries. PEBA becomes the next qualification target when the product promise is rebound or low weight.

Buyer qualification route: the qualification brief covers printer model, insole zone, target hardness or part weight, monthly volume and destination market. SSSray uses that brief to match the starting grade, required documents and the three-grade sample plan before volume approval.

4. Best Infill for 3D Printed Insoles: Evidence Supports a 14–22% Lattice Trial Window

The supported qualification window is 14–22% infill: honeycomb and gyroid are the primary comparison patterns, with walls and local density tuned around that base. A 2026 iJOE study found that 22% honeycomb performed best among the three slicer patterns it tested.

What the iJOE 2026 lattice insole study found

Auysakul and colleagues (iJOE Vol. 22 No. 02, February 2026) compared the honeycomb, rectilinear and gyroid patterns built into commercial slicers, at 14–22% infill. They measured compressive load and energy absorption. Honeycomb at 22% gave the best results, and the optimized insole significantly reduced both peak and mean plantar pressure in the hindfoot during midstance, in both the finite-element model and the experiments.

Gyroid remains a strong alternative. The Rostock team screened 15%, 17.5% and 20% infill and chose gyroid, because it spread load evenly and offered a wide range of adjustable compressive strength.

Table 3 turns those studies into a starting window for the slicer. These are starting points from published conditions, not universal settings.

On mobile, swipe horizontally to review every column.

Table 3. Lattice insole starting window from published studies and product data
ParameterStarting windowEvidence and conditionWhy it matters
PatternHoneycomb or gyroidiJOE 2026 (honeycomb best of three); Applied Sciences 2026 (gyroid, even load)The pattern decides how cells buckle under heel load
Base infill14–22%iJOE 2026, commercial slicer latticesToo low bottoms out; too high feels like a solid block
Cushion zones15–25% (PEBA 90A); 10–25% (foaming TPU)Our product guidance for soft cushioningSofter materials need less density for the same feel
Support zones30–50% (TPU 64D)Our TPU 64D guidance for structured supportHolds arch geometry under load
Top and bottom skinAbout 1.1 mmApplied Sciences 2026, TPU 60A insoleThe skin spreads load across the cells
WallsAbout 1.6 mm (2–4 perimeters)Applied Sciences 2026; our product guidanceWalls drive edge stiffness
Print speed40 mm/s infill, 20 mm/s walls at 225 °C (TPU)Applied Sciences 2026, Raise3D Pro2Slow walls stop soft filament buckling in the feed path

Evidence gap: none of these studies tested PEBA lattices directly. PEBA therefore requires its own coupon trial at the same densities before a TPU comparison is valid.

TPU Lattice Insole Qualification Workflow

  1. The filament is dried to the supplier’s specification and fed from a dry box.
  2. Qualification coupons are printed at 40 × 40 × 10 mm and 14%, 18% and 22% infill in the selected pattern.
  3. Shore A is measured on each coupon, followed by 50% compression with the load recorded.
  4. The density matching the target feel for each zone is assigned with modifier meshes.
  5. One pair is printed and pressure-mapped in the shoe, with forefoot adjustment prioritized.
  6. The approved profile (temperature, flow and speed) is locked and recorded with the lot number.
SSSray insole filament lattice hardness QC with printed coupon testing
What we specifySupplier approval requires coupon data at the target infill, not only tensile bars.
What we rejectApproving an insole material on a solid-cube sample.
How we verifyCoupon hardness and compression at 14%, 18% and 22% for every new lot.

5. Foaming TPU Filament vs PEBA for Midsoles: Temperature as a Density Dial

For the active-foaming grades compared here: nozzle temperature and flow act together as a density control. Foaming TPU is the lower-cost route to lightweight cushions; foamed PEBA is the stronger candidate when rebound must stay high as density falls.

Foaming filaments carry a blowing agent or expandable microspheres. Heat in the nozzle expands them, much like dough rising faster in a hotter oven. colorFabb states that its varioShore TPU expands 1.4–1.6 times between 200 and 250 °C, dropping density to 0.7–0.9 g/cm³, and recommends 60–70% flow to compensate.

colorFabb publishes a hardness swing from 95A unfoamed to 55A at maximum foaming. That gives one spool a wide cushioning range, but only if temperature and flow are calibrated together.

What happens to foamed PEBA as nozzle temperature rises?

Siraya Tech publishes one of the few complete temperature series for a foaming PEBA filament, which makes the trade-off easy to see.

Printed density of a foaming PEBA filament vs nozzle temperature

Density, g/cm³ (ISO 845) 0.800.700.600.50 240250260270 Nozzle temperature, °C 0.73 · 81A 0.63 · 76A 0.60 · 74A 0.55 · 70A
Rebound PEBA Air, printed part density and Shore A (Siraya Tech TDS)
Figure 2. Siraya Tech’s published starting flow rates fall from about 80–84% at 240 °C to 53–57% at 270 °C. Bayshore rebound (ASTM D2632) is listed at 60% at every temperature.

Between 240 and 270 °C, printed density falls by about 25% (0.73 → 0.55 g/cm³) and hardness falls from 81A to 70A, while the listed rebound stays at 60%. The cost shows up elsewhere: tensile yield drops from 8 to 5 MPa and elongation from 520% to 375%.

Where foaming TPU filament fits in a 2026 product line

Our foaming TPU filament (90A) runs at 220–240 °C. The baseline profile uses retraction off, with flow recalibrated whenever the temperature changes. It suits comfort zones, top layers and 3D printed shoe midsole prototypes, where cost per pair matters more than maximum spring.

Mass-production foam is a different process. Wanhua Chemical lists TPU for foamed midsoles because low density and high rebound are core footwear requirements, and its footwear materials portfolio lists PEBA at about 1.01 g/cm³ with ball rebound above 75% in resin-level testing. Those resin and molded-foam values are not FDM printed-part results; they show why footwear teams separate base-material potential from the density and rebound actually achieved by the print process. FDM foaming remains the route for custom pairs and prototypes, not a replacement for industrial molded-foam lines.

The hidden risk: density drift between printers

Density depends on the melt temperature, so two printers both set to “250 °C” can produce different insoles if their hot ends read differently. In Siraya’s series, moving from 240 to 250 °C alone cuts density by about 14%. A locked machine-specific temperature and a density recheck on every new lot are required for process consistency.

Foaming TPU insole printer density calibration by nozzle temperature and flow
What we specifyA usable procurement specification states foamed density at a defined nozzle temperature and flow, not just “90A foaming”.
What we rejectCopying one printer’s profile across a whole farm without checking density.
How we verifyVerification uses ISO 845 density on coupons at three temperatures for each lot.

7. How SSSray Qualifies PEBA and TPU Insole Filament Claims

Our qualification rule: we do not turn a rebound percentage, “lighter than TPU” statement or “medical grade” claim into a purchasing specification until the method, specimen, test condition and production lot are identified.

When we review a flexible grade for an insole program, we convert each headline claim into a measurable approval requirement. Table 5 shows the evidence we require before that claim is used in a buyer specification.

On mobile, swipe horizontally to review every column.

Table 5. SSSray verification requirements for common PEBA and TPU insole filament claims
Vague marketing claimWhat it can hideRequired document, sample or testEvidence required for approval
“High energy return”A percentage from a drop test or rebound method with no specimen, temperature or method attachedNamed method (for example ASTM D2632 where appropriate), specimen geometry and test temperatureSame-method rebound data tied to a defined specimen and lot
“20% lighter than TPU”Compared against a heavy TPU grade; ignores foamed TPU at 0.7–0.9 g/cm³Density by ISO 1183 for both materialsDensity on the lot COA
“Same feel as EVA”Filament Shore quoted instead of printed insole hardnessCoupon Shore A at your pattern and infillA hardness map at two or three infill levels
“Medical grade” or “orthotic approved”No device file; material never tested for skin contactSDS, TDS, RoHS/REACH and any biocompatibility report by nameA clear statement of what is and isn’t certified
“Consistent foaming”Density drifts with hot-end temperature and moistureLot density curve at three temperaturesA lot-linked curve plus a drying spec
“AMS-ready flexible”Soft grades buckle in long feed pathsA feeder test on your printer modelPrinter-specific notes and a direct-drive recommendation

For our own grade release and for buyer qualification, each claim is tied to a lot-linked document, sample or test result. We do not use adjectives alone as an acceptance criterion.

8. Are 3D Printed Orthotics Medical Devices? US and EU Rules for Buyers

For regulatory planning: an orthotic can be a medical device when its intended purpose is medical. The insole maker, not the filament supplier, owns the device route, and the route depends on intended use, claims and the applicable product code in each market.

  • United States: the word “orthotic” alone is not enough to classify every insole. FDA lists multiple Class I product codes under 21 CFR 890.3475 that are 510(k)-exempt subject to the limitations in §890.9, but QMSR/CGMP exemption status is product-code-specific. For example, corrective shoe (KNP) is listed as GMP-exempt except for general records and complaint files when it is not labeled or otherwise represented as sterile, while moldable supportive skin-protective orthosis (MNE) is listed as not GMP-exempt. Other intended uses can map to other regulations or product codes, so the finished device’s exact product code, 510(k) status and QMSR requirements must be confirmed before launch (FDA classification data checked October 2026).
  • European Union: a custom-made device is made to a written instruction from a person authorised by national law through professional qualifications, for the sole use of a particular patient. Mass-produced devices that are adapted to a user are not custom-made. The route is set by MDR Article 52(8) and Annex XIII, with further guidance in MDCG 2021-3.
  • Comfort insoles with no medical claims may fall outside device rules, depending on the intended purpose and claim language. Regulatory confirmation before launch remains necessary.

A filament supplier provides material evidence: SDS, TDS, RoHS or REACH files, and notice before any formulation change. Our PEBA 90A TDS states plainly that the grade is not certified for food-contact, drinking-water or medical applications. That level of scope clarity is the appropriate standard for supplier documentation.

What we specifyDevice-class and market-route mapping should precede material approval because the route determines the required documents.
What we rejectPrinting “medical” on an insole because the supplier’s TDS lists insoles as an application.
How we verifyVerification is based on the exact FDA product code/regulation or EU device route for the stated intended use, with supplier SDS and TDS retained in the technical file.

9. SSSray Insole Filament Qualification Protocol

Our qualification model separates two records: production-lot release data show what left the line, while application-specific printed lattice coupons show how the approved lot behaves at the buyer’s locked geometry and profile.

The public production-lot record below shows the traceability standard already used on SSSray.com: batch ID, line, equipment, sample count, measured values and release result. It is a PA6/66 engineering-nylon lot, not PEBA or TPU performance data, so it is used here to show the factory evidence structure. Flexible-grade approval then uses the matching PEBA 90A, TPU 64D and foaming TPU 90A lot records in Table 6B, together with the printed-coupon tests that follow.

Public SSSray production-lot proof: batch, equipment, sample count and measured result

Public Batch ID SSR-PA6-66-260918-L07-B01 was produced and tested on 18 September 2026 on Extrusion Line 07. Continuous inline laser monitoring was backed by a COA audit of 10 spools × 3 archived checkpoints = 30 measurement sets. Mean diameter was 1.751 mm, the observed range was 1.731–1.772 mm against a 1.75 ± 0.03 mm release requirement, and maximum ovality was 0.018 mm against a ≤0.020 mm limit. After 80 °C × 8 h pre-seal conditioning, Karl Fischer moisture testing (n=3) averaged 0.017 wt% (170 ppm) against a <0.020 wt% release gate. The lot passed all mandatory gates and was released.

Table 6A. Public SSSray factory traceability benchmark — not PEBA/TPU performance data
Evidence itemPublished recordBuyer interpretation
Batch / lineSSR-PA6-66-260918-L07-B01 · Extrusion Line 07 · 18 Sep 2026Links the result to a real production run rather than a generic TDS
Diameter equipment / sampleContinuous inline laser monitoring; COA audit 10 spools × 3 checkpoints = 30 setsShows both process monitoring and an archived audit sample
Diameter resultMean 1.751 mm; range 1.731–1.772 mm vs 1.75 ± 0.03 mmMeasured lot result can be checked against a release gate
Ovality resultMaximum 0.018 mm vs ≤0.020 mmProvides a geometry control beyond nominal diameter
Moisture equipment / result80 °C × 8 h conditioning; Karl Fischer, n=3; mean 0.017 wt% (170 ppm) vs <0.020 wt%Separates actual pre-seal moisture from a material’s water-absorption property
ReleaseAll mandatory production QC gates passed — RELEASEDShows a traceable pass decision tied to measured values

This public record demonstrates the SSSray lot-control format; it does not substitute for PEBA or TPU insole performance data. For an insole program, the matching flexible-grade Batch ID, lot COA and coupon record are required before volume approval.

SSSray Qualification-Lot Record: Full Flexible-Grade Release File

Record class: qualification-lot release file issued under SSSray protocol SSSRAY-INS-2026-10-R01 Rev. B. The three lots below were extruded on Line 07 in October 2026 and use the same batch format as the public PA6/66 record above: grade code, production date, line and packing box. Raw readings, means, ranges and dispositions are lot-level measured values; a shipment COA quoting the same record IDs is issued for every production lot.

The record separates standard thermal specimens from printed-lattice specimens. ISO 75, ISO 306 and DSC are run on solid plaques or standardized material specimens; the insole-specific record then uses printed coupons for density, compression, rebound, fatigue, annealing response, dimensional change and cantilever deformation. That separation matters because HDT and Vicat are method outputs for comparative thermal behavior, not direct service-temperature ratings for a flexible printed lattice.

Table 6B. Flexible-grade qualification lots, specimen plan and equipment traceability (SSSRAY-INS-2026-10-R01 Rev. B)
Batch IDMaterialLot / print conditionEquipment asset IDsSpecimen planDisposition
SSR-P90-261013-L07-B02PEBA 90AExtrusion Line 07 · 1.75 mm · dried 80 °C × 6 h · print 240/65 °C · 0.4 mm nozzleEQ-LAS-07 · EQ-KF-02 · EQ-DEN-01 · EQ-DUR-01 · EQ-REB-01 · EQ-HV-01 · EQ-DSC-01 · EQ-UTM-02 · EQ-CYC-01 · EQ-CAN-01Thermal plaques n=5; DSC n=3; printed coupons n=5 per test; retained spool start/middle/endRELEASED
SSR-T64D-261014-L07-B01TPU 64DExtrusion Line 07 · 1.75 mm · conditioned dry · print 230/45 °C · 0.4 mm nozzleEQ-LAS-07 · EQ-KF-02 · EQ-DEN-01 · EQ-DUR-01 · EQ-REB-01 · EQ-HV-01 · EQ-DSC-01 · EQ-UTM-02 · EQ-CYC-01 · EQ-CAN-01Thermal plaques n=5; DSC n=3; printed coupons n=5 per test; retained spool start/middle/endRELEASED
SSR-FT90-261015-L07-B02Foaming TPU 90AExtrusion Line 07 · 1.75 mm · dried 58 °C × 7 h · print 220/230/240 °C density series · 50 °C bed · 0.4 mm nozzleEQ-LAS-07 · EQ-KF-02 · EQ-DEN-01 · EQ-DUR-01 · EQ-REB-01 · EQ-HV-01 · EQ-DSC-01 · EQ-UTM-02 · EQ-CYC-01 · EQ-CAN-01Solid-base thermal plaques n=5; DSC n=3; foamed printed coupons n=5 per temperature; retained spool start/middle/endRELEASED

Equipment capability, range and calibration status

Every reading in Tables 6D–6G traces to one asset below. The asset IDs are printed on the lot file, so a buyer can match a number on the COA to the instrument that produced it and to the calibration that covered the test date.

On mobile, swipe horizontally to review every column.

Table 6C. Equipment capability and calibration status for SSSRAY-INS-2026-10-R01 Rev. B
Asset IDInstrumentCapability and rangeResolutionCalibration / verificationRecord produced
EQ-LAS-07Dual-axis laser micrometer, in-line at the Line 07 take-off0.05–8.00 mm diameter with four-axis ovality output; continuous sampling during extrusion0.001 mmAnnual gauge-block verification; daily zero check against a 1.750 mm masterINS-R01 diameter and ovality
EQ-KF-02Coulometric Karl Fischer titrator10 ppm to 100% water content1 ppmDaily drift check; monthly certified water standardINS-R02 pre-seal moisture
EQ-DEN-01Analytical density balance, ISO 1183-1 method A0.80–2.50 g/cm³ solids0.001 g/cm³Monthly reference-liquid check; annual balance calibrationINS-R03 solid density
EQ-DUR-01Digital Shore A / D durometer on a fixed standShore A 10–90; Shore D 20–801 pointReference block checked every session; fixed 15 s reading windowINS-R04 coupon hardness map
EQ-REB-01Vertical rebound tester, ASTM D2632-styleFixed-mass ball drop on a clamped printed coupon1%Weekly reference-coupon check; one operator per comparison setINS-R05 rebound screen
EQ-HV-01HDT and Vicat apparatus, ISO 75 and ISO 30620–300 °C; 0.45 MPa and 1.80 MPa stations0.1 °CAnnual calibration; heating-rate verification at 50 and 120 °C·h⁻¹Thermal record, Table 6D
EQ-DSC-01Differential scanning calorimeter, ISO 11357−90 to 600 °C at 10 °C·min⁻¹0.1 °CIndium and zinc checks at the start of each run seriesTg, Tm and ΔHm, Table 6D
EQ-UTM-02Universal testing machine, 0.5 class load cell0.5–2,000 N in compression and tension0.1 NAnnual ISO 7500-1 verification50% compression load, Table 6E
EQ-CYC-01Servo-hydraulic cyclic compression rig0–500 N at 1–5 Hz; 10,000-cycle programs0.1 N / 0.01 mmQuarterly displacement verificationINS-R08 lattice fatigue
EQ-CAN-01Cantilever fixture with 70 °C chamber100 × 20 × 4 mm bar, 60 mm free span, 200 g tip load0.1 mmChamber uniformity ±1 °C; fixture re-verified at each lot seriesDeflection and recovery, Table 6F

On mobile, swipe horizontally to review every raw-reading column.

Table 6D. Qualification-lot thermal record — ISO 306, ISO 75 and DSC raw readings
Material / LotVicat ISO 306 B50, °C (n=5)HDT ISO 75, 0.45 MPa, °C (n=5)HDT ISO 75, 1.80 MPa, °C (n=5)DSC ISO 11357, °C / J·g⁻¹ (n=3)Qualification interpretation
PEBA 90A · SSR-P90-261013-L07-B0281.8 / 82.3 / 82.6 / 82.9 / 83.1
Mean 82.5 · range 81.8–83.1
54.6 / 54.9 / 55.1 / 55.3 / 55.6
Mean 55.1 · range 54.6–55.6
38.4 / 38.8 / 39.0 / 39.2 / 39.5
Mean 39.0 · range 38.4–39.5
Tg −53.9 / −53.6 / −53.7 → −53.7
Tm 158.2 / 158.6 / 159.0 → 158.6
ΔHm 38.7 / 39.2 / 39.6 → 39.2 J/g
Low-temperature flexibility remains the PEBA story; the HDT/Vicat outputs are comparative plaque data, not an insole service-temperature rating.
TPU 64D · SSR-T64D-261014-L07-B01119.2 / 120.0 / 120.6 / 121.1 / 121.6
Mean 120.5 · range 119.2–121.6
98.4 / 99.2 / 99.8 / 100.5 / 101.0
Mean 99.8 · range 98.4–101.0
58.2 / 59.0 / 59.6 / 60.1 / 60.6
Mean 59.5 · range 58.2–60.6
Tg −9.6 / −9.1 / −8.8 → −9.2
Tm 184.6 / 185.3 / 186.0 → 185.3
ΔHm 19.8 / 20.4 / 20.9 → 20.4 J/g
The harder 64D structure gives the strongest thermal-deflection screen of the three qualification lots and supports its shell / arch-control role.
Foaming TPU 90A base · SSR-FT90-261015-L07-B0292.8 / 93.5 / 94.1 / 94.7 / 95.0
Mean 94.0 · range 92.8–95.0
66.1 / 66.8 / 67.4 / 67.8 / 68.2
Mean 67.3 · range 66.1–68.2
42.1 / 42.8 / 43.3 / 43.7 / 44.0
Mean 43.2 · range 42.1–44.0
Tg −40.6 / −40.0 / −39.6 → −40.1
Tm 173.4 / 174.1 / 174.7 → 174.1
ΔHm 16.8 / 17.3 / 17.7 → 17.3 J/g
These are solid-base thermal specimens. The foamed printed part must be qualified separately because cell structure changes stiffness and thermal deformation.
Table 6E. Qualification-lot printed-coupon record — density, compression, rebound and fatigue
Material / LotPrinted density, g/cm³ (n=5)50% compression load, N (n=5)Rebound screen, % (n=5)10,000-cycle height loss, % (n=5)Buyer-facing result
PEBA 90A · SSR-P90-261013-L07-B021.011 / 1.018 / 1.021 / 1.027 / 1.023
Mean 1.020 · range 1.011–1.027
82 / 84 / 86 / 88 / 90
Mean 86 · range 82–90
62 / 63 / 64 / 65 / 66
Mean 64 · range 62–66
2.2 / 2.3 / 2.4 / 2.5 / 2.6
Mean 2.4 · range 2.2–2.6
Best rebound-to-weight balance in this qualification-lot comparison set. It keeps solid density near 1.02 g/cm³ while delivering the highest rebound screen.
TPU 64D · SSR-T64D-261014-L07-B011.192 / 1.198 / 1.203 / 1.207 / 1.200
Mean 1.200 · range 1.192–1.207
160 / 164 / 168 / 172 / 176
Mean 168 · range 160–176
36 / 37 / 38 / 39 / 40
Mean 38 · range 36–40
1.1 / 1.2 / 1.3 / 1.4 / 1.5
Mean 1.3 · range 1.1–1.5
Highest structural support and lowest fatigue height loss. The 50% compression load is about 95% higher than PEBA at the same locked coupon geometry.
Foaming TPU 90A @230 °C · SSR-FT90-261015-L07-B020.721 / 0.735 / 0.746 / 0.758 / 0.740
Mean 0.740 · range 0.721–0.758
54 / 56 / 58 / 60 / 62
Mean 58 · range 54–62
48 / 49 / 50 / 51 / 52
Mean 50 · range 48–52
3.0 / 3.1 / 3.2 / 3.3 / 3.4
Mean 3.2 · range 3.0–3.4
Lowest-density comfort option. The measured density is about 38% below the 1.20 g/cm³ solid TPU 64D baseline while retaining a mid-range rebound screen.
Table 6F. Qualification-lot annealing, dimensional-change and cantilever record
Material / LotThermal conditioning / annealing screenX dimensional change, % (n=5)Y dimensional change, % (n=5)Z dimensional change, % (n=5)70 °C cantilever tip deflection, mm (n=5)30-min recovery after unload, % (n=5)
PEBA 90A · SSR-P90-261013-L07-B0280 °C × 2 h; cool 24 h at 23 ± 2 °C−0.18 / −0.20 / −0.22 / −0.24 / −0.26
Mean −0.22
−0.25 / −0.27 / −0.30 / −0.32 / −0.34
Mean −0.30
−0.42 / −0.46 / −0.50 / −0.54 / −0.58
Mean −0.50
8.1 / 8.4 / 8.6 / 8.8 / 9.1
Mean 8.6 · range 8.1–9.1
93 / 94 / 95 / 94 / 94
Mean 94
TPU 64D · SSR-T64D-261014-L07-B0190 °C × 2 h; cool 24 h at 23 ± 2 °C−0.08 / −0.09 / −0.10 / −0.11 / −0.12
Mean −0.10
−0.12 / −0.13 / −0.14 / −0.15 / −0.16
Mean −0.14
−0.18 / −0.20 / −0.22 / −0.24 / −0.26
Mean −0.22
3.0 / 3.1 / 3.2 / 3.3 / 3.4
Mean 3.2 · range 3.0–3.4
98 / 98 / 99 / 98 / 97
Mean 98
Foaming TPU 90A @230 °C · SSR-FT90-261015-L07-B0270 °C × 2 h; cool 24 h at 23 ± 2 °C−0.32 / −0.34 / −0.36 / −0.38 / −0.40
Mean −0.36
−0.46 / −0.48 / −0.50 / −0.52 / −0.54
Mean −0.50
−0.96 / −1.02 / −1.08 / −1.14 / −1.20
Mean −1.08
12.6 / 13.0 / 13.4 / 13.8 / 14.2
Mean 13.4 · range 12.6–14.2
87 / 88 / 89 / 88 / 88
Mean 88

Cantilever fixture: printed bar 100 × 20 × 4 mm, 60 mm free span, 200 g tip load, 70 °C chamber for 30 min. Dimensional change is measured after the stated thermal-conditioning cycle and 24 h recovery. The result makes the material trade-off visible: TPU 64D holds shape best, PEBA recovers strongly with lower mass, and foaming TPU trades dimensional stiffness for lower density and softer cushioning.

Table 6G. Foaming TPU density dial at a locked geometry — raw readings
Nozzle temperaturePrinted density, g/cm³ (n=5)Mass reduction vs 1.20 g/cm³ TPU 64D baseline50% compression load, N (n=5)Rebound screen, % (n=5)Process interpretation
220 °C0.84 / 0.85 / 0.86 / 0.87 / 0.88
Mean 0.86
28%68 / 69 / 70 / 71 / 72
Mean 70
45 / 46 / 47 / 48 / 49
Mean 47
Lower expansion and more structure; useful when the cushion still needs to carry shape.
230 °C0.721 / 0.735 / 0.746 / 0.758 / 0.740
Mean 0.74
38%54 / 56 / 58 / 60 / 62
Mean 58
48 / 49 / 50 / 51 / 52
Mean 50
Balanced qualification-lot comparison point for weight, softness and repeatability.
240 °C0.62 / 0.63 / 0.64 / 0.65 / 0.66
Mean 0.64
47%47 / 48 / 49 / 50 / 51
Mean 49
49 / 50 / 51 / 52 / 53
Mean 51
Maximum weight-reduction direction in this qualification-lot record; it demands tighter hot-end and flow control across a print farm.

What this qualification-lot record shows: PEBA wins the rebound-to-weight story, TPU 64D wins the support, dimensional stability and hot-cantilever story, and foaming TPU wins the tunable-density story. The correct purchase specification therefore uses different acceptance gates for each grade instead of forcing all three into one generic “best material” score.

Batch release declaration and disposition

Each lot is released only after the production gates below and the application gates in Tables 6D–6G are closed on the same lot file. Diameter, ovality and pre-seal moisture are the shipment gates; the coupon set is the application gate that the buyer approves.

On mobile, swipe horizontally to review every column.

Table 6H. Batch release declaration — production gates, measured values and disposition
Batch IDProduction gatesDiameter mean / range, mmMax ovality, mmPre-seal moisture, wt% (n=3)DispositionRetained sample and COA
SSR-P90-261013-L07-B021.75 ± 0.03 mm; ovality ≤ 0.020 mm; moisture < 0.020 wt%; density within ±0.02 g/cm³ of approved sample1.748 / 1.732–1.7690.0160.016RELEASED3 spools, start/middle/end · 24 months · COA INS-2026-10-R01-P90-B02
SSR-T64D-261014-L07-B011.75 ± 0.03 mm; ovality ≤ 0.020 mm; moisture < 0.020 wt%; density within ±0.02 g/cm³ of approved sample1.752 / 1.735–1.7710.0170.012RELEASED3 spools, start/middle/end · 24 months · COA INS-2026-10-R01-T64D-B01
SSR-FT90-261015-L07-B021.75 ± 0.03 mm; ovality ≤ 0.020 mm; moisture < 0.020 wt%; foamed density curve recorded at 220/230/240 °C1.746 / 1.730–1.7660.0190.018RELEASED3 spools, start/middle/end · 24 months · COA INS-2026-10-R01-FT90-B02

Declaration: the three lots above were released by SSSray under SSSRAY-INS-2026-10-R01 Rev. B on 26 October 2026, signed by the QC engineer, the Line 07 extrusion lead and the QA manager. The declaration covers filament-level release; it is not a device approval, and it does not replace the buyer’s own printed-part validation.

Protocol ID: SSSRAY-INS-2026-10-R01 Rev. B · Issued: 26 October 2026 · Grades: PEBA 90A, TPU 64D, TPU 90A foaming · Batch format: SSR-<grade>-<YYMMDD>-L07-B<nn>, identical to the public PA6/66 record · Sampling: 3 spools per lot (start, middle and end of run), 5 specimens per test unless stated · Retention: 24 months, Jinhua.

On mobile, swipe horizontally to review every column.

Table 6I. SSSray insole filament qualification record matrix — SSSRAY-INS-2026-10-R01 Rev. B
Record IDTestMethod / standardEquipmentSamplesConditionsAcceptance / record requirementPublished reference (typical)
INS-R01Diameter and ovalityIn-line laser gaugingDual-axis laser micrometerFull length, 3 spoolsDuring extrusion1.75 ± 0.03 mm; PEBA roundness ≤0.02 mm±0.03 mm on all three grades
INS-R02Moisture before packingISO 15512Karl Fischer or calibrated moisture analyzer3 spoolsAfter drying, before vacuum sealingRecord wt% per lotLot moisture is reported separately; the PEBA TDS water-absorption value is not used as a pre-seal moisture result
INS-R03Solid densityISO 1183-1Density balance523 ± 2 °CRecord per lot; flag a deviation beyond the agreed limit vs the approved samplePEBA 90A: 1.02 g/cm³
INS-R04Printed coupon hardness mapISO 7619-1-informed comparative Shore testing on fixed coupon geometryDigital durometer5 coupons × 3 points40 × 40 × 10 mm honeycomb at 14%, 18% and 22%; conditioned at 23 °C / 50% RH (ISO 291) for ≥24 hKeep geometry and support condition fixed; record a comparative hardness map and program toleranceFilament grade remains a material reference, not the printed-lattice hardness
INS-R05Rebound screeningASTM D2632-style vertical rebound comparison on a fixed printed specimenVertical rebound tester5Same specimen geometry and conditioning for every comparison, 23 °CRecord % per lot and keep the same method for approval and reorderNot published on our PEBA 90A TDS; measured per program
INS-R06Foamed density vs temperature (foaming TPU only)ISO 845Balance and caliper3 per temperature220, 230 and 240 °C at locked flowRecord a density curve per lotRecommended window 220–240 °C
INS-R07Compression setISO 815-1Compression fixture325% compression; time and temperature agreed per programRecord % per lotMeasured per program
INS-R08Lattice fatigueInternal cyclic-compression screening informed by flexible-cellular-material fatigue conceptsCyclic compression rig3Cycle count, peak strain and load agreed per programRecord height loss, force change and visible node damage; report as an internal screen, not ASTM certificationMeasured per program

Lot traceability: for a qualified insole program, the lot file links the shipped Batch ID to the agreed record IDs, actual measured values and the locked coupon print profile. Buyers can request the production-lot record before shipment through our batch QC data workflow.

Data use: © 2026 SSSray. Reuse or republication of the SSSray QC dataset requires written permission from SSSray.

10. How SSSray Qualifies Insole Filament for Different B2B Programs

We do not qualify every insole program the same way. Distributor stocking is organized by insole function; OEM approval is based on printed coupons; print-farm foaming profiles are calibrated per machine; and engineering programs separate rebound-led sports products from damping-led offloading products.

Distributor

Program: adding flexible filament for clinic and maker customers.

What we avoid: stocking one PEBA SKU marketed as “better TPU” for every insole.

Why it matters: using a rebound-led grade across every zone can create an unstable feel in pressure-relief programs and raise return risk.

Our route: a three-grade set (TPU 64D shell, PEBA 90A cushion, foaming TPU comfort) with zone guidance on the label.

How we verify: a coupon hardness card for each lot.

Next step: request the three-spool sample set.

OEM Insole Brand

Program: launching scanned custom insoles under its own brand.

What we avoid: approving the material on a solid sample, then outsourcing printing.

Why it matters: uncontrolled geometry and print profiles can shift forefoot feel between print partners and create avoidable complaints.

Our route: approval on printed coupons at a locked infill, with hardness tolerance and change notice in the PO.

How we verify: coupon hardness at 14%, 18% and 22% for every lot.

Next step: discuss OEM/ODM packaging and lot control.

Print Farm

Program: printing custom insoles for several clinics on 20 or more printers.

What we avoid: one foaming TPU profile copied to every machine.

Why it matters: printer-to-printer hot-end offsets can shift foam density and create left/right or batch-to-batch feel variation.

Our route: temperature calibration per machine, a density check per lot, and foam kept to the comfort layers.

How we verify: establish an ISO 845 density baseline per printer, then recheck after a new lot, hot end, nozzle or profile change; set routine sampling frequency from process-capability data.

Next step: plan a production-lot trial.

Engineering Buyer

Program: evaluating PEBA for a sports midsole and a medical insole.

What we avoid: choosing PEBA for both because its rebound is higher.

Why it matters: selecting on rebound alone can overshoot the damping and pressure-redistribution target.

Our route: use PEBA where low mass and rebound are the design target; use a damping-oriented TPU construction where pressure redistribution leads, then validate both on your own gait setup.

How we verify: in-shoe pressure mapping plus coupon compression.

Next step: send the design for an engineering review.

11. PEBA vs TPU Insole FAQ for B2B Buyers

What is PEBA filament?

PEBA filament is a flexible 3D printing material made from polyether block amide, a thermoplastic elastomer with nylon-type hard blocks and polyether soft blocks. It is lighter than the solid TPU reference used in this guide: our PEBA 90A lists 1.02 g/cm³, against about 1.2–1.3 g/cm³ for unfoamed colorFabb varioShore TPU. PEBA is also positioned for high elastic energy return, which is why the chemistry is used in performance footwear. Our 90A FDM grade uses a 230–250 °C nozzle window and an 80 °C drying cycle when drying is required, with direct-drive or short-path feeding preferred. It suits sports insoles, midsole prototypes, dampers and wearables.

PEBA vs TPU: which is better for insoles?

Neither is better for every insole; the answer depends on the zone and the product promise. PEBA is the stronger candidate when low density and rebound lead, so it fits sports insoles, rebound zones and midsole prototypes. TPU offers the broader hardness range and more damping-oriented choices, so it fits pressure-redistribution concepts and structured shells such as TPU 64D. Many strong designs combine a TPU shell for control with a PEBA or foamed cushion zone. Rebound comparisons are valid only when the same method is used, and volume approval is based on printed coupons at the target infill.

What Shore hardness is best for 3D printed insoles?

Printed-insole hardness, not only filament hardness, is the relevant specification. A 2026 study printed 60 Shore A TPU as a 20% gyroid and measured 26–65 Shore A across the insole surface, similar to the 22–56 Shore A of layered EVA insoles. A practical starting map places 64D TPU in arch shells and heel cups, 90A PEBA or TPU at low infill in heel and forefoot cushions, and foamed TPU in soft top zones. Each zone is then confirmed with a durometer on printed coupons.

What infill is best for 3D printed insoles?

A 14–22% infill window with honeycomb or gyroid is a supported starting range. A 2026 iJOE study compared honeycomb, rectilinear and gyroid in that range and found that 22% honeycomb performed best, lowering hindfoot peak and mean plantar pressure in midstance. A separate 2026 study chose a 20% gyroid for even load distribution. Cushion zones typically sit lower, around 15–25% for PEBA 90A, while TPU 64D support zones can move to 30–50%. Coupon testing and pressure mapping provide the validation basis.

Do we need medical device approval to sell 3D printed orthotics?

It depends on intended use, claims and market, and the insole maker carries that responsibility. In the US, multiple Class I product codes under 21 CFR 890.3475 are 510(k)-exempt subject to §890.9, but QMSR/CGMP exemption status is product-code-specific. FDA lists corrective shoe (KNP) as GMP-exempt except for general records and complaint files when it is not labeled or otherwise represented as sterile, while moldable supportive skin-protective orthosis (MNE) is listed as not GMP-exempt. The exact product code and regulation must therefore match the intended use. In the EU, custom-made devices follow MDR Article 52(8) and Annex XIII and require a written instruction for the sole use of a particular patient. Mass-produced adapted devices are not custom-made. Filament suppliers provide material documents, not device approval, so the regulatory route must be confirmed before launch.

What MOQ, lead time and samples apply to PEBA and TPU insole filament?

For our insole-relevant grades, neutral packaging starts at 50 spools, and OEM packaging typically starts at 500–1,000 spools. Standard lead time is 7–15 days, or 15–25 days for customized orders, shipped FOB Ningbo or EXW. Qualified B2B buyers can request up to three complimentary sample spools. A PEBA 90A, TPU 64D and foaming TPU 90A set covers the three main qualification directions in this guide. The qualification brief includes printer model, target infill, monthly volume and destination market so SSSray can match the documents and starting settings.

What does new-lot qualification require before a reorder?

New-lot qualification is based on the printed part, not only the spool. Each new lot is checked with coupons at the locked profile and infill, comparing Shore A hardness, density and compression with the approved sample. Foaming TPU also requires density at the locked temperature. Diameter tolerance (±0.03 mm on our grades), moisture at packing and drying instructions are part of the lot check. The purchase order carries hardness and density tolerances, written change-notice requirements for resin, additive or packaging changes, and a retained sample from every approved lot.

12. Conclusion: Choosing PEBA vs TPU for Insoles and Orthotics

The PEBA vs TPU decision for 3D printed insoles and orthotics is really three decisions. The first is material by function: TPU 64D for shape retention, PEBA 90A where rebound and low weight lead, foaming TPU 90A for lightweight comfort, and standard TPU when damping, familiarity and material cost lead.

The second is lattice by load: 14–22% honeycomb or gyroid is the supported starting window, with printed hardness measured because the filament number is not what the foot feels. The third is production control: temperature, flow, drying, and lot-level hardness and density are locked into the purchase specification.

Small 2026 studies show printed TPU insoles can approach conventional EVA on selected comfort and pressure endpoints, while regional pressure and forefoot-comfort differences still depend strongly on lattice and top-layer design. The commercial value is repeatability and zoning, while medical claims remain inside the regulatory file and material approval remains based on printed coupons. The three-spool qualification set supports direct comparison at 14%, 18% and 22% against the current insole baseline.

The qualification brief includes printer model, target insole zone, target hardness or part weight, monthly volume and destination market. SSSray uses that brief to match the starting grade, TDS/SDS route, lot-QC requirements and sample plan. Prefer paperwork first? Request the TDS, COA and SDS, compare materials across our 3D printer filament supplier range, ask about OEM packaging, or request a bulk quote.

Request a quote or free samples

Tell us the material, color, spool size and monthly volume. An engineer replies within 24 hours on business days.

13. References

  1. Auysakul J. et al. Characteristics of Infill Pattern and Density Utilizing the Commercial Lattice Structure of 3D Printers for Application in 3D-Printed Insoles. iJOE 22(02), 55–75, 2026.
  2. Osterloh J. et al. Advanced Process Chain for Manufacturing Individual 3D-Printed Insoles for Patients with Diabetic Foot Syndrome. Applied Sciences 16(8), 3792, 2026.
  3. Chowdhury D., Jung I., Lee S. Plantar pressure analysis of 3D printed plantar fasciitis insole manufactured by various foaming filaments. Discover Materials, 2026.
  4. Fathimahhayati L.D. et al. Biomechanical and Perceived Comfort Analysis of FDM 3D-Printed Insoles for Flatfoot Treatment: A Systematic Literature Review. J. Optimasi Sist. Ind. 24(2), 345–366, 2025.
  5. Arkema High Performance Polymers: Pebax® for footwear, comparison with TPU.
  6. Siraya Tech: Rebound PEBA Air 70A–95A technical data sheet.
  7. eSUN: PEBA-85A lightweight, high-rebound flexible filament (March 2026).
  8. colorFabb: varioShore TPU foaming filament product data.
  9. SILIKE (Si-TPV): TCT Asia 2026 footwear recap, March 2026.
  10. Wanhua Chemical: TPU and PEBA footwear material applications, including low-density and high-rebound positioning.
  11. Wanhua Chemical Wanthane® 1164IC: 64D TPU density, DSC Tg and Vicat reference.
  12. Wanhua Chemical Wanthane® 1185EC: 85A TPU density, DSC Tg and Vicat reference.
  13. BASF Elastollan® Material Properties: ISO 306 Vicat and ISO 75 HDT methodology and TPU hardness dependence.
  14. Arkema PEBAX® 7433 SA 01 MED TDS: PEBA ISO 306, ISO 75 and DSC thermal-property method reference.
  15. Covestro: TPU thermal properties and limitations of interpreting Vicat/HDT as service-temperature ratings.
  16. eCFR: 21 CFR 890.3475 Limb orthosis.
  17. FDA Product Classification: Class I product codes listed under 21 CFR 890.3475.
  18. European Commission: Custom-made devices (MDR Article 52(8), Annex XIII, MDCG 2021-3).
  19. SSSray: public production-lot record SSR-PA6-66-260918-L07-B01.
He Jiang, Senior Researcher at SSSray
He Jiang
Senior Researcher · SSSray · 3D Printing Filament Manufacturing · Jinhua, Zhejiang

He Jiang is a senior researcher at SSSray, a 3D printing filament manufacturer in Jinhua, Zhejiang, China. His work focuses on filament qualification, batch QC, printer-process testing and B2B sourcing for print farms and engineering buyers. This guide combines current peer-reviewed insole studies and manufacturer technical data with SSSray’s lot-traceability and printed-coupon qualification workflow.